MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Protactinium, Pa
Categories: Metal; Nonferrous Metal; Pure Element

Material Notes: Malleable and Ductile. Properties vary with isotope.

Physical Form: Shiny Metal; Tetragonal or Cubic

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 15.43 g/cc
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 231.0359231.03588 - 1995
Atomic Number 91
X-ray Absorption Edge 0.11028 ÅK
 0.58748 ÅLI
 0.61064 ÅLII
 0.74138 ÅLIII
Electronegativity 1.5Pauling
Ionic Radius 0.890 ÅCrystal Ionic Radius for Valence +5
 0.980 ÅCrystal Ionic Radius for Valence +4
 1.13 ÅCrystal Ionic Radius for Valence +3
 
Mechanical PropertiesOriginal ValueComments
Bulk Modulus 157 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000150 ohm-cm
Magnetic Susceptibility 190emu/mol
Critical Superconducting Temperature 1.40 K
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 12.3 J/g
CTE, linear 9.90 µm/m-°C
@Temperature 30.0 - 700 °C
Specific Heat Capacity 0.09912 J/g-°CGas
Thermal Conductivity 47.0 W/m-K
Melting Point 1552 - 1592 °C
Heat of Formation 0.000 kJ/molCrystal
 607 kJ/molGas
 
Component Elements PropertiesOriginal ValueComments
Protactinium, Pa 100 %
 
Descriptive Properties
CAS Number7440-73-3

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Neptunium, Np
Polonium, Po
Promethium, Pm
Americium, Am
Meitnerium, Mt

AMEPa00 / 79

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.