MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Pacific Silver Fir Wood
Categories: Wood and Natural Products; Wood; Softwood

Key Words: Abies Amabilis; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.370 g/ccGreen, based on volume
 0.430 g/cc12% moisture content, based on volume
 
Mechanical PropertiesOriginal ValueComments
Hardness, Wood Indentation 1379 NGreen
 3025 N12% moisture content
Tensile Strength at Break 240 psiGreen, perpendicular to grain
Modulus of Elasticity 1420 ksiGreen
 1760 ksi12% moisture content
Modulus of Rupture 6.40 ksiGreen
 11.0 ksi12% moisture content
Compressive Strength 220 psiGreen, perpendicular to grain
 450 psi12% moisture content, perpendicular to grain
 3140 psiGreen, parallel to grain
 6410 psi12% moisture content, parallel to grain
Shear Strength 750 psiGreen, parallel to grain
 1220 psi12% moisture content, parallel to grain
Impact 21Impact bending in inches, green
 24Impact bending in inches, 12% moisture content
Work to Maximum Load 6.00 in-lb/in³Green
 9.30 in-lb/in³12% moisture content
 
Thermal PropertiesOriginal ValueComments
Shrinkage 4.4 %Radial, from green to oven dry, US origin
 9.2 %Tangential, from green to oven dry, US origin
 13 %Volumetric, from green to oven dry, US origin

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Fir, Subalpine
Silver Fir Wood
Boxelder Wood
Douglas-fir Plywood
Hem-Fir Wood

PTSU006 / 71448

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.