MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Alcoa Deltalloy® 4032-T651 Aluminum
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 4000 Series Aluminum Alloy

Material Notes: Weldability = B; Stress Corrosion Cracking Resistance = B; General Corrosion Resistance = C (A = best; E = worst). General 4032 characteristics and uses: Good machinability and drilling characteristics when using single point or multi-spindle screw machines. Excellent surface finish using polycrystalline or carbide tooling. Superior wear resistance, eliminated the need for hard coat anodizing. High strength, low thermal expansion.

Uses: Master brake cylinders, transmission valves, copier parts, bushings for rack and pinion steering systems, sound recording devices, bearings and hydraulic applications, forged pistons.

Data supplied by the manufacturer, Alcoa.

Key Words: Aluminum 4032-T651; 4032-T651 Aluminium; UNS A94032; Alcoa, Aluminum Company of America; AA4032-T651
Vendors: Eagle Alloys Corporation is a leading supplier of quality metals and alloys. Our staff prides itself on working fast, efficiently and courteously to get you the information you need. Call (800) 237-9012 or visit www.EagleAlloys.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.68 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 120500 kg load/10 mm ball
Hardness, Knoop 150Estimated from Brinell
Hardness, Rockwell A 46.8Estimated from Brinell
Hardness, Rockwell B 75Estimated from Brinell
Hardness, Vickers 136Estimated from Brinell
Tensile Strength, Ultimate >= 359 MPa
Tensile Strength, Yield >= 331 MPa
Elongation at Break 4.0 %
Modulus of Elasticity 79.0 GPa
Fatigue Strength 110 MPa
@# of Cycles 5.00e+8
completely reversed; R. R. Moore Machine and specimen.
Machinability 70 %0-100 Scale (A=90; B=70; C=50; D=30; E=10)
Shear Strength 262 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000450 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 19.4 µm/m-°C
@Temperature 20.0 - 100 °C
average
Thermal Conductivity 138 W/m-K
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 85 %
Chromium, Cr <= 0.10 %
Copper, Cu 0.50 - 1.3 %
Iron, Fe <= 1.0 %
Magnesium, Mg 0.80 - 1.3 %
Nickel, Ni 0.50 - 1.3 %
Silicon, Si 11 - 13.5 %
Zinc, Zn <= 0.25 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 4032-T6
Alcoa Deltalloy® 4032-T86 Aluminum
Aluminum 4032-O
Aluminum 6061-T6; 6061-T651
Materion AMC4632 Aluminum Silicon Alloy, T6

NALCOA00 / 14743

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.