Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 4.17 g/cc | 4.17 g/cc |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 51.3 | 51.3 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 390 @Load 0.0999 kg | 390 @Load 0.220 lb |
Modulus of Elasticity | 75.7 GPa | 11000 ksi |
Modulus of Rigidity | 29.4 GPa | 4260 ksi |
Poissons Ratio | 0.287 | 0.287 |
Abrasion | 521 | 521 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 11.7 µm/m-°C @Temperature -30.0 - 70.0 °C | 6.50 µin/in-°F @Temperature -22.0 - 158 °F |
| 13.5 µm/m-°C @Temperature 100 - 300 °C | 7.50 µin/in-°F @Temperature 212 - 572 °F |
Thermal Conductivity | 0.624 W/m-K @Temperature 35.0 °C | 4.33 BTU-in/hr-ft²-°F @Temperature 95.0 °F |
Transformation Temperature, Tg | 571 °C | 1060 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.57252 @Wavelength 2325.42 nm | 1.57252 @Wavelength 2325.42 nm |
| 1.57631 @Wavelength 1970.09 nm | 1.57631 @Wavelength 1970.09 nm |
| 1.58045 @Wavelength 1529.58 nm | 1.58045 @Wavelength 1529.58 nm |
| 1.58426 @Wavelength 1128.64 nm | 1.58426 @Wavelength 1128.64 nm |
| 1.58557 @Wavelength 1013.98 nm | 1.58557 @Wavelength 1013.98 nm |
| 1.58791 @Wavelength 852.11 nm | 1.58791 @Wavelength 852.11 nm |
| 1.58954 @Wavelength 768.19 nm | 1.58954 @Wavelength 768.19 nm |
| 1.59105 @Wavelength 706.52 nm | 1.59105 @Wavelength 706.52 nm |
| 1.59255 @Wavelength 656.27 nm | 1.59255 @Wavelength 656.27 nm |
| 1.59298 @Wavelength 643.85 nm | 1.59298 @Wavelength 643.85 nm |
| 1.59337 @Wavelength 632.8 nm | 1.59337 @Wavelength 632.8 nm |
| 1.59514 @Wavelength 589.29 nm | 1.59514 @Wavelength 589.29 nm |
| 1.59522 @Wavelength 587.56 nm | 1.59522 @Wavelength 587.56 nm |
| 1.59732 @Wavelength 546.07 nm | 1.59732 @Wavelength 546.07 nm |
| 1.60134 @Wavelength 486.13 nm | 1.60134 @Wavelength 486.13 nm |
| 1.60184 @Wavelength 479.99 nm | 1.60184 @Wavelength 479.99 nm |
| 1.60549 @Wavelength 441.57 nm | 1.60549 @Wavelength 441.57 nm |
| 1.60612 @Wavelength 435.835 nm | 1.60612 @Wavelength 435.835 nm |
| 1.61008 @Wavelength 404.656 nm | 1.61008 @Wavelength 404.656 nm |
| 1.61681 @Wavelength 365.015 nm | 1.61681 @Wavelength 365.015 nm |
Abbe Number | 67.37 | 67.37 |
| 67.74 | 67.74 |
Optical Dispersion | 0.002665 | 0.002665 |
| 0.003015 | 0.003015 |
| 0.00396 | 0.00396 |
| 0.004338 | 0.004338 |
| 0.004528 | 0.004528 |
| 0.004761 | 0.004761 |
| 0.004782 | 0.004782 |
| 0.006988 | 0.006988 |
| 0.007411 | 0.007411 |
| 0.008787 | 0.008787 |
| 0.008866 | 0.008866 |
| 0.010681 | 0.010681 |
| 0.010904 | 0.010904 |
| 0.014961 | 0.014961 |
Transmission, Visible | 98 % @Thickness 10.0 mm, Wavelength 380 nm | 98 % @Thickness 0.394 in, Wavelength 380 nm |
| 98.8 % @Thickness 10.0 mm, Wavelength 390 nm | 98.8 % @Thickness 0.394 in, Wavelength 390 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 420 nm | 98.9 % @Thickness 0.394 in, Wavelength 420 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 440 nm | 98.9 % @Thickness 0.394 in, Wavelength 440 nm |
| 99.1 % @Thickness 10.0 mm, Wavelength 400 nm | 99.1 % @Thickness 0.394 in, Wavelength 400 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 460 nm | 99.2 % @Thickness 0.394 in, Wavelength 460 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 480 nm | 99.4 % @Thickness 0.394 in, Wavelength 480 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 500 nm | 99.6 % @Thickness 0.394 in, Wavelength 500 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 650 nm | 99.6 % @Thickness 0.394 in, Wavelength 650 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 700 nm | 99.6 % @Thickness 0.394 in, Wavelength 700 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 600 nm | 99.7 % @Thickness 0.394 in, Wavelength 600 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 550 nm | 99.8 % @Thickness 0.394 in, Wavelength 550 nm |
IR Transmittance | 98.3 % @Thickness 10.0 mm, Wavelength 2400 nm | 98.3 % @Thickness 0.394 in, Wavelength 2400 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 2200 nm | 98.9 % @Thickness 0.394 in, Wavelength 2200 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 2000 nm | 99.2 % @Thickness 0.394 in, Wavelength 2000 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 800 nm | 99.5 % @Thickness 0.394 in, Wavelength 800 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 900 nm | 99.5 % @Thickness 0.394 in, Wavelength 900 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 1800 nm | 99.5 % @Thickness 0.394 in, Wavelength 1800 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 1000 nm | 99.6 % @Thickness 0.394 in, Wavelength 1000 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 1200 nm | 99.7 % @Thickness 0.394 in, Wavelength 1200 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 1400 nm | 99.7 % @Thickness 0.394 in, Wavelength 1400 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 1600 nm | 99.7 % @Thickness 0.394 in, Wavelength 1600 nm |
UV Transmittance | 18 % @Thickness 10.0 mm, Wavelength 310 nm | 18 % @Thickness 0.394 in, Wavelength 310 nm |
| 35 % @Thickness 10.0 mm, Wavelength 320 nm | 35 % @Thickness 0.394 in, Wavelength 320 nm |
| 54 % @Thickness 10.0 mm, Wavelength 330 nm | 54 % @Thickness 0.394 in, Wavelength 330 nm |
| 72 % @Thickness 10.0 mm, Wavelength 340 nm | 72 % @Thickness 0.394 in, Wavelength 340 nm |
| 84 % @Thickness 10.0 mm, Wavelength 350 nm | 84 % @Thickness 0.394 in, Wavelength 350 nm |
| 91.7 % @Thickness 10.0 mm, Wavelength 360 nm | 91.7 % @Thickness 0.394 in, Wavelength 360 nm |
| 95.8 % @Thickness 10.0 mm, Wavelength 370 nm | 95.8 % @Thickness 0.394 in, Wavelength 370 nm |
|
Descriptive Properties |
---|
Acid Resistance, Powder Method, RA(P) | 1 |
CCI | 0.00 B |
| 0.32 G |
| 0.32 R |
coloring, λ 5 | 295 |
coloring, λ 80 | 355 |
Coloring, Internal Transmission λ 0.05 | 302 |
Coloring, Internal Transmission λ 0.80 | 347 |
Knoop Hardness Class | 4 |
Ohara Code d | 595677 |
Ohara Code e | 597674 |
Phosphate Resistance, PR | 4.1 |
Photoelastic Constant (ß) | 0.51 |
Water Resistance, RW(P) | 1 |
Weathering Resistance (Surface Method) W(S)max | 2 |
Yield Point, At (°C) | 596 |