Network Polymers NPP Nylon 66G13L
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, 10% Glass Fiber Filled
Material Notes:
Description:
Nylon
Information provided by Network Polymers Inc.
A. Schulman has acquired Network Polymers.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.22
g/cc
1.22
g/cc
ASTM D792
Water Absorption
1.0 %
1.0 %
24 hours Immersion; ASTM D570
Linear Mold Shrinkage, Flow
0.0050
cm/cm
0.0050
in/in
1/8 in bar; ASTM D955
Linear Mold Shrinkage, Transverse
0.0090
cm/cm
0.0090
in/in
ASTM D955
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell R
122
122
ASTM D785
Tensile Strength at Break
103
MPa
15000
psi
ASTM D638
Elongation at Break
2.0 - 4.0 %
2.0 - 4.0 %
ASTM D638
Flexural Strength
148
MPa
21500
psi
ASTM D790
Flexural Modulus
4.83
GPa
700
ksi
ASTM D790
Izod Impact, Notched
0.374
J/cm
0.700
ft-lb/in
1/8 in specimen; ASTM D256
Tensile Impact Strength
126
kJ/m²
60.0
ft-lb/in²
ASTM D1822
Thermal Properties
Metric
English
Comments
Melting Point
255
°C
491
°F
ASTM D789
Deflection Temperature at 1.8 MPa (264 psi)
240
°C
464
°F
0.125 in bar; ASTM D648
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Clariant Renol PA123G13 Nylon 66, 13% Glass Fiber, Impact Modified, Heat Stabilized, Lubricated
Hybrid Plastics MS0825 Nanoreinforced® POSS® Polyamide 6
A. Schulman Diamond NYLON 66 Natural
BASF Ultramid® B24 NSD 05 PA6
Domo Domamid® 33 ABH Polyamide 6.6
PDIAM162 / 30000
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.