MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Toyobo Celstran® PP-GF20-0553 XLE PP, 20% Long Glass Reinforced
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 20% Glass Fiber Filler

Material Notes: Product Description: Material code according to ISO 1043-1: PP copolymer reinforced with 20% long glass fibers. Black. The fibers are chemically coupled to the polypropylene matrix. The pellets are cylindrical and normally as well as the embedded fibers 10 mm long. Low odor grade, not suggest to use mold release or lubricants in molding.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Filler/Reinforcement: Glass Fiber

Use: Automotive Applications

Features: Good Heat Resistance; Low Emissions; Low Warpage

Use: Automotive Applications

Automotive Specifications: DAIMLER DBL 5405.70; GWM MP01 LG-01; LI AUTO INC Q/LIA 5 3100 50 2019 V1; SAIC MOTO SMTC-5-310-041

Forms: Pellets

Processing Method: Injection Molding

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.02 g/cc0.0368 lb/in³ISO 1183
Maximum Moisture Content 0.200.20
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 84.1 MPa12200 psiISO 527-2/5
Elongation at Break 2.6 %2.6 %ISO 527-2/5
Tensile Modulus 4.50 GPa653 ksiISO 527-1
Flexural Strength 135 MPa19600 psiISO 178
Flexural Modulus 4.60 GPa667 ksiISO 178
Charpy Impact Unnotched 5.46 J/cm²26.0 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 1.99 J/cm²9.50 ft-lb/in²ISO 179/1eA
 
Processing PropertiesMetricEnglishComments
Processing Temperature 230 - 250 °C446 - 482 °FHot Runner
Feed Temperature 20.0 - 50.0 °C68.0 - 122 °FInjection
Rear Barrel Temperature 200 - 220 °C392 - 428 °F
Middle Barrel Temperature 210 - 230 °C410 - 446 °F
Front Barrel Temperature 220 - 250 °C428 - 482 °F
Nozzle Temperature 220 - 250 °C428 - 482 °F
Zone 4 220 - 250 °C428 - 482 °FInjection
Melt Temperature 220 - 250 °C428 - 482 °F
Mold Temperature 30.0 - 70.0 °C86.0 - 158 °F
Drying Temperature 90.0 - 100 °C194 - 212 °F
Dry Time 2.00 hour2.00 hour
Back Pressure <= 3.00 MPa<= 435 psi
Screw Speed  25 rpm
@Thickness 76.2 mm
25 rpm
@Thickness 3.00 in
 35 rpm
@Thickness 55.9 mm
35 rpm
@Thickness 2.20 in
 50 rpm
@Thickness 40.6 mm
50 rpm
@Thickness 1.60 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCQ6250 / 310943

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.