MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay FM® 6555-1 Ester Syntactic Core
Categories: Polymer; Adhesive; Thermoset; Acrylic/Cyanoacrylate Adhesive

Material Notes: FM® 6555-1 is a cyanate ester syntactic core material. It was designed as a cost and weight saving alternative in the manufacture of thin, stiffness critical composite panels for low dielectric applications and satellite structures. FM 6555-1 syntactic core is based on CYCOM® 5575-2 glass and quartz cyanate ester prepregs, FM 2555 and FM 2525 structural film adhesives and FM 313-27C syntactic paste, providing a compatible family of products. FM 6555-1 is available in sheet or roll form (availability in roll form is dependent on product thickness).

Features & Benefits:

  • One of a family of compatible products based on second-generation cyanate ester chemistry
  • Significantly improved electrical properties versus epoxy and BMI systems
  • Excellent mechanical properties
  • Service temperature from -70 to 350°F (-57 to 177°C) wet
  • Simple thermoset processing
  • Product and application patents received
Applications:
  • Thin composite panels for low dielectric applications and space structures where weight and/or cost are critical

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.513 - 0.577 g/ccCured; ASTM D792
Volatiles 1.0 %
@Temperature 177 °C,
Time 3600 sec
ASTM D3530
Viscosity >= 5000 cP
@Temperature 105 °C
 7500 cP
@Temperature 93.0 °C
 17000 cP
@Temperature 80.0 °C
 130000 cP
@Temperature 60.0 °C
Storage Temperature -18.0 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 70 - 73ASTM D2240
Tensile Strength 2600 psidry; ASTM D638
Flexural Strength 2800 psiASTM D790
Compressive Strength 4000 psi
@Temperature 150 °C
wet; ASTM D1621
 6500 psi
@Temperature 150 °C
dry; ASTM D1621
 7500 psi
@Temperature 25.0 °C
dry; ASTM D1621
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 1.6ASTM D2520
Dielectric Loss Index 0.0050
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 177 °C
Minimum Service Temperature, Air -57.0 °C
Glass Transition Temp, Tg 200 °CASTM D1356
 
Processing PropertiesOriginal ValueComments
Cure Time 3.00 hour
@Pressure 0.276 MPa,
Temperature 177 °C
Gel Time 8.00 min
@Temperature 17.0 °C
Hot plate
 19.0 min
@Temperature 150 °C
Hot plate
Shelf Life 6.00 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Hexcel® HexPly® 954-3 Curing Cyanate Resin
Park Aerospace Nelcote® V-376 Cyanate Ester Epoxy Prepregs, 7781 E-Glass Reinforced
Hexcel® HexPly® 954-3A Curing Cyanate Resin
CRG Industries Advantic™ 40 Syntactic Foam
CRG Industries Advantic™ 30 Syntactic Foam

PCYTED044 / 180346

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.