MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Unitika P-1001A Engineering Plastic
Categories: Polymer; Thermoplastic; Polyarylate

Material Notes: P series resins are resins succeeding the characteristics of the neat polymer, U100, and improved in flowability and optical properties. Among many super engineering plastics, the resins are few transparent polymer alloys that have heat resistance. The heat stable P-series resins have variations different in heat resistance in the range from 150 to 175°C. There are few transparent heat resistant resins among super engineering plastics, and thus P series resins are valuable. The resins have favorable weather resistance, and in particular, the P1001 resin is approved by SAE Standard (J576 and J578) and FMVSS Standard (108).Making the most of these characteristics, the resins may be used, for example, as the lenses for automobile lamps. High flow type resins, P1001A, and P3001S, are also available for thin molding products.

Characteristics:

  • Transparent, heat resistant, deflection temperature under load: 150 to 175°C (under a great load of 1.8 MPa)
  • High weather resistance
  • High creep resistant
  • High dimensional stability
  • High impact strength

Information provided by Unitika Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.21 g/ccASTM D792
Water Absorption 0.26 %
@Thickness 3.17 mm,
Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 3.00 mm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 123ASTM D785
Tensile Strength at Break 69.0 MPaASTM D638
Elongation at Break 50 %ASTM D638
Flexural Strength 81.0 MPaASTM D790
Flexural Modulus 2100 MPaASTM D790
Izod Impact, Notched 196 J/m
@Thickness 3.17 mm
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.00e+14 ohm-cmASTM D257
Dielectric Constant 3.0
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 787 V/milASTM D149
Dissipation Factor 0.010
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 127 secASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear 62.0 µm/m-°CASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 175 °CASTM D648
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 310 - 330 °C
Middle Barrel Temperature 330 - 350 °C
Front Barrel Temperature 350 - 370 °C
Nozzle Temperature 350 - 370 °C
Mold Temperature 120 - 140 °Cactual surface temp
Drying Temperature 140 °C
Dry Time 6.00 - 24.0 hour
Back Pressure 0.490 - 1.47 MPagage pressure

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Unitika U-100 Engineering Plastic
Unitika P-3001 Engineering Plastic
Unitika P-3001S Engineering Plastic
Unitika UG-100-20 Engineering Plastic
NHEP Spectron™ E5469 Nylon 66, 33% Glass Fiber

PUNITIK879 / 177899

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.