MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chemours Viton® GF-600S with 3phr, DCP-40KE Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • Cures exceptionally fast to a high state of cure
  • Exhibits improved mold release/mold fouling properties compared to Viton® GF
  • Exhibits improved mold flow, less shear sensitivity, and lower extruder die swell for a ~65 Mooney FKM
  • Exhibits excellent physical properties with high elongation, both original and aged
  • Exhibits similar heat, fluids, and low temperature resistance compared to Viton® GF
  • Exhibits excellent compression set resistance with short (2 hr) or no postcure

Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 71No Postcure; ASTM D2240
 752 hours Postcure; ASTM D2240
Tensile Strength at Break 14.8 MPaNo Postcure; ASTM D412
 18.5 MPa2 hours Postcure; ASTM D412
Tensile Stress at Strain 0.800 MPa
@Strain 10 %
No Postcure; ASTM D412
 1.10 MPa
@Strain 10 %
2 hours Postcure; ASTM D412
Elongation at Break 256 %2 hours Postcure; ASTM D412
 281 %No Postcure; ASTM D412
100% Modulus 0.00510 GPa
@Strain 100 %
No Postcure; ASTM D412
 0.00670 GPa
@Strain 100 %
2 hours Postcure; ASTM D412
Compression Set 10 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, postcured; ASTM D1414
 14 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, no postcure; ASTM D1414
 20 %
@Temperature 200 °C,
Time 252000 sec
O-Rings, postcured; ASTM D1414
 21 %
@Temperature 200 °C,
Time 252000 sec
O-Rings no postcure; ASTM D1414
 
Thermal PropertiesOriginal ValueComments
Glass Transition Temp, Tg -5.60 °C
 
Processing PropertiesOriginal ValueComments
Processing Temperature 177 °C
@Time 421 sec
Cure
 232 °C
@Time 7200 sec
Postcure
 
Component Elements PropertiesOriginal ValueComments
Fluorine, F 70 %Uncompounded Viton
 
Descriptive Properties
Compound NumberA08-06
Formulation as Tested100GF-600S
 3Diak 7 (TAIC)
 3Zinc Oxide
 30MT Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chemours Viton® GFLT-600S with ZnO Fluoroelastomer Compound
Chemours Viton® GBLT-600S Fluoroelastomer Compound
Chemours Viton® GF-600S Fluoroelastomer Compound
Chemours Viton® GF-600S with 3phr, DBPH50-HP Fluoroelastomer Compound
Chemours Viton® GBLT-600S with 5-MT Black Fluoroelastomer Compound

PDVC9837 / 170478

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.