MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Polynt DISTITRON® 183 CAV5F Unsaturated Polyester Resin
Categories: Polymer; Thermoset; Polyester, TS

Material Notes: Unsaturated polyester resin in styrene, Isophthalic

Appearance: Yellow - Light - Transparent

Main resin characteristics: Clear, unaccelerated

Main applications: Production of Gelcoat

Molding information: Mix with fillers and/or additives

Curing cycle: 24h at 23°C + 2h at 100°C + 1h at 100°C

Information provided by Polynt Composites.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.11 g/cc
Solids Content 60 - 64 %MT-CU001C
Brookfield Viscosity 480 - 570 cPsp 2 rpm 20; MT-CUT25V
 
Chemical PropertiesOriginal ValueComments
Acid Value 11 - 18[mgKOH/g]; MT-CU001I
 
Mechanical PropertiesOriginal ValueComments
Hardness, Barcol 40ASTM D 2583
Tensile Strength 80.0 MPaISO 527
Elongation at Break 4.2 %ISO 527
Tensile Modulus 3600 MPaISO 527
Flexural Strength 140 MPaISO 178/B
Flexural Modulus 3500 MPaISO 178/B
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °CISO 75 -2A
 
Processing PropertiesOriginal ValueComments
Gel Time 16.0 - 22.0 min
@Temperature 23.0 °C
Reactivity, at 23°C + 1% Co 1% + 1% MEKP50; RS.08.G
Shelf Life 6.00 Monthin the dark; MT-CU002S
 
Descriptive Properties
Peak Exotherm185-215°CRS.08.G; Reactivity, at 23°C + 1% Co 1% + 1% MEKP50

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Polynt DISTITRON® 100 SV3 Unsaturated Polyester Resin
Polynt DISTITRON® 100 BSX15 Unsaturated Polyester Resin
Polynt HUP 15/28 RN-colour Class A
Polynt DISTITRON® 822 S Unsaturated Polyester Resin
Polynt DISTITRON® 183 CS Unsaturated Polyester Resin

PPOLYN9293 / 231888

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.