MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI Type 416Se Stainless Steel, tempered and cold drawn wire 6.4 mm diameter
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Key Words: UNS S41623, AMS 5610, ASME SA194, ASTM A194, ASTM A314, ASTM A473, ASTM A511, ASTM A581, ASTM A582, MIL SPEC MIL-S-862, SAE J405 (51416Se)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 92
Tensile Strength, Ultimate 620 MPa
Tensile Strength, Yield 550 MPa
@Strain 0.2 %
Elongation at Break 10 %gage length is 4 times diameter
Modulus of Elasticity 200 GPa
Poissons Ratio 0.20Calculated
Shear Modulus 83.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000570 ohm-cm
@Temperature 20.0 °C
 0.000108 ohm-cm
@Temperature 650 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.90 µm/m-°C
@Temperature 0.000 - 100 °C
 11.0 µm/m-°C
@Temperature 0.000 - 315 °C
 11.5 µm/m-°C
@Temperature 0.000 - 540 °C
 11.7 µm/m-°C
@Temperature 0.000 - 650 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 24.9 W/m-K
@Temperature 100 °C
 28.7 W/m-K
@Temperature 500 °C
Melting Point 1480 - 1530 °C
Solidus 1480 °C
Liquidus 1530 °C
Maximum Service Temperature, Air 675 °CContinuous Service
 760 °CIntermittent
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.15 %
Chromium, Cr 13 %
Iron, Fe 84 %
Manganese, Mn <= 1.25 %
Phosphorus, P <= 0.060 %
Selenium, Se >= 0.15 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.060 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
416 Stainless Steel, annealed wire 6.4 mm diameter
AISI Type 416Se Stainless Steel, tempered bar
416 Stainless Steel, tempered bar
416 Stainless Steel, tempered and cold drawn bar 25 mm diameter
416 Stainless Steel, annealed bar

MQ416SJ / 13058

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.