MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay LTM® 26EL Epoxy with Woven Glass Fiber Laminate
Categories: Polymer; Thermoset; Epoxy; Epoxy/Glass SMC

Material Notes: LTM26 series prepregs are low to medium viscosity epoxy resin matrices formulated to cure at low initial cure temperatures. These prepregs can be used to manufacture components by autoclave, press or vacuum bag molding techniques. After post-cure, these resins are suitable for service temperatures up to 115°C (239°F) dry or 90°C (194°F) wet

Features & Benefits:

  • Out life between 2 and 5 days at 21°C (0°F)
  • 12 months storage at -18°C (0°F)
  • Low initial cure temperatures from 50 to 60°C(122 to 140°F)
  • Service temperatures under load up to 115°C (239°F)
  • Excellent mechanical properties, equivalent to many 120°C (248°F) curing prepreg systems
  • Adhesion to foam core materials
  • High quality components can be made from low cost and low temperature molds
  • Rapid cure capability between 80°C (176°F) and 120°C (248°F)
Product Variants:
LTM26ELB- Black pigmented version of LTM26EL
LTM26ELFR- Fire-retarded version of LTM26EL, passing JAR25.853 vertical burn
LTM26ELFRB-Black pigmented version of LTM26ELFR
LTM26ELFS- Low smoke (DIN5510, M1 compliant) variant of this resin system, see PDS1035

Property data for LTM26EL/300g/m2 8 harness satin (epoxy saline) woven glass fiber laminates; Cure cycle: 14 hours at 60°C (140°F), 6.2 bar (90 psi); Post-cure: 0.5 hour at 120°C (248°F)

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.18 g/ccCured Resin, 1 hr at 120°C
Storage Temperature -18.0 °C
 
Mechanical PropertiesOriginal ValueComments
Flexural Strength 10200 psi
@Temperature 21.0 °C
0° Orientation, Cured; CRAG 200
 63100 psi
@Temperature 100 °C
0° Orientation, Post-Cured, wet; CRAG 200
 75800 psi
@Temperature 100 °C
0° Orientation, Post-Cured; CRAG 200
 79300 psi
@Temperature 50.0 °C
0° Orientation, Post-Cured, wet; CRAG 200
 89500 psi
@Temperature 21.0 °C
0° Orientation, Post-Cured, wet; CRAG 200
 91000 psi
@Temperature 50.0 °C
0° Orientation, Post-Cured; CRAG 200
 92000 psi
@Temperature 21.0 °C
0° Orientation, Cured, wet; CRAG 200
 95100 psi
@Temperature 50.0 °C
0° Orientation, Cured; CRAG 200
 95700 psi
@Temperature 21.0 °C
0° Orientation, Post-Cured; CRAG 200
Flexural Modulus 20.0 GPa
@Temperature 100 °C
0° Orientation, Post-Cured, wet; CRAG 200
 21.0 GPa
@Temperature 100 °C
0° Orientation, Post-Cured; CRAG 200
 21.0 GPa
@Temperature 50.0 °C
0° Orientation, Post-Cured; CRAG 200
 22.0 GPa
@Temperature 50.0 °C
0° Orientation, Post-Cured, wet; CRAG 200
 22.0 GPa
@Temperature 21.0 °C
0° Orientation, Cured; CRAG 200
 23.0 GPa
@Temperature 21.0 °C
0° Orientation, Cured, wet; CRAG 200
 24.0 GPa
@Temperature 21.0 °C
0° Orientation, Post-Cured, wet; CRAG 200
 25.0 GPa
@Temperature 21.0 °C
0° Orientation, Post-Cured; CRAG 200
 26.0 GPa
@Temperature 50.0 °C
0° Orientation, Cured; CRAG 200
Shear Strength 4350 psi
@Thickness 2540 mm
0° Interlaminar, Post-cured, wet; ASTM D2344
 5370 psi
@Thickness 2540 mm
0° Interlaminar, Post-cured; ASTM D2344
 5950 psi
@Thickness 1270 mm
0° Interlaminar, Post-cured, wet; ASTM D2344
 6380 psi
@Thickness 1270 mm
0° Interlaminar, Cured; ASTM D2344
 6380 psi
@Thickness 1270 mm
0° Interlaminar, Post-cured; ASTM D2344
 6530 psi
@Thickness 533 mm
0° Interlaminar, Cured, wet; ASTM D2344
 7250 psi
@Thickness 533 mm
0° Interlaminar, Post-cured, wet; ASTM D2344
 7400 psi
@Thickness 533 mm
0° Interlaminar, Cured; ASTM D2344
 7540 psi
@Thickness 533 mm
0° Interlaminar, Post-cured; ASTM D2344
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 90.0 °CWet, Post-Cure Required
 115 °CDry, Post-Cure Required
Glass Transition Temp, Tg 75.0 °CDMA E' onset, 8 hrs at 60°C
 130 °CDMA E' onset, 8 hrs at 60°C+1 hr at 120°C
 
Processing PropertiesOriginal ValueComments
Processing Temperature 60.0 °CCure Temp. Optimum
 50.0 - 100 °CCure Temp. Range
 120 °C
@Time 3600 sec
Recommended Post-Cure
Gel Time 11.0 min
@Temperature 100 °C
 22.0 min
@Temperature 90.0 °C
 44.0 min
@Temperature 80.0 °C
 90.0 min
@Temperature 70.0 °C
 135 min
@Temperature 65.0 °C
 200 min
@Temperature 60.0 °C
 300 min
@Temperature 55.0 °C
 450 min
@Temperature 50.0 °C
Shelf Life 12.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Abatron ClearStrip™ Stripper for Paint, Varnish, Coatings; Gel
ASTM A897 Grade 5 (230-185-00 or 230-185-01) Austempered Ductile Iron
Calcium Sulfate Dihydrate, CaSO4-2H2O
Fibre Glast 72 White Gel Coat
Gypsum (CaSO4 - 2H2O)

PCYTED140d / 193492

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.