SABIC XENOY™ 5220U PC+PBT (Americas)
Categories:
Polymer
;
Thermoplastic
;
Polycarbonate (PC)
;
Polycarbonate/Polybutylene Terephthalate (PBT) Blend, Unreinforced
Material Notes:
Unreinforced PBT+PC Alloy. Impact Modified. Improved retention of mechanical properties under UV exposure. Excellent low temperature impact and chemical resistance.
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.20
g/cc
1.20
g/cc
ASTM D792
1.21
g/cc
1.21
g/cc
ASTM D792
Density
1.22
g/cc
0.0441
lb/in³
ISO 1183
Water Absorption
0.50 %
0.50 %
23°C/sat; ISO 62
Moisture Absorption
0.150 %
0.150 %
23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow
0.0080
-
0.010
cm/cm
@Thickness 3.20 mm
0.0080
-
0.010
in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse
0.0080
-
0.011
cm/cm
0.0080
-
0.011
in/in
SABIC method
Melt Flow
15
g/10 min
@Load 5.00 kg,
Temperature 250 °C
15
g/10 min
@Load 11.0 lb,
Temperature 482 °F
cm³/10 min; ISO 1133
16
g/10 min
@Load 5.00 kg,
Temperature 250 °C
16
g/10 min
@Load 11.0 lb,
Temperature 482 °F
ISO 1133
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
50.0
MPa
7250
psi
50 mm/min; ISO 527
51.0
MPa
7400
psi
50 mm/min; ASTM D638
Tensile Strength, Yield
50.0
MPa
7250
psi
50 mm/min; ISO 527
53.0
MPa
7690
psi
50 mm/min; ASTM D638
Elongation at Break
120 %
120 %
50 mm/min; ASTM D638
120 %
120 %
50 mm/min; ISO 527
Elongation at Yield
4.0 %
4.0 %
50 mm/min; ISO 527
4.0 %
4.0 %
50 mm/min; ASTM D638
Tensile Modulus
2.05
GPa
297
ksi
1mm/min; ISO 527
2.25
GPa
326
ksi
50 mm/min; ASTM D638
2.25
GPa
326
ksi
5 mm/min; ASTM D638
Flexural Yield Strength
80.0
MPa
11600
psi
2 mm/min; ISO 178
84.0
MPa
12200
psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus
2.00
GPa
290
ksi
2 mm/min; ISO 178
2.03
GPa
294
ksi
1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched
7.10
J/cm
13.3
ft-lb/in
ASTM D256
2.99
J/cm
@Temperature -40.0 °C
5.60
ft-lb/in
@Temperature -40.0 °F
ASTM D256
5.30
J/cm
@Temperature -30.0 °C
9.93
ft-lb/in
@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO)
50.0
kJ/m²
23.8
ft-lb/in²
80*10*4; ISO 180/1A
30.0
kJ/m²
@Temperature -30.0 °C
14.3
ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched
5.50
J/cm²
26.2
ft-lb/in²
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy
60.0
J
44.3
ft-lb
ASTM D3763
Electrical Properties
Metric
English
Comments
Arc Resistance
120
-
180
sec
120
-
180
sec
ASTM D495
Comparative Tracking Index
400
-
600
V
400
-
600
V
UL 746A
Hot Wire Ignition, HWI
15
-
30
sec
15
-
30
sec
UL 746A
High Amp Arc Ignition, HAI
>=
120
arcs
>=
120
arcs
UL 746A
High Voltage Arc-Tracking Rate, HVTR
0.000
-
10.0
mm/min
0.000
-
0.394
in/min
UL 746A
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
95.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
52.8
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
95.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
52.8
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow
90.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
50.0
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
90.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
50.0
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)
107
°C
@Thickness 6.40 mm
225
°F
@Thickness 0.252 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
75.0
°C
167
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
84.0
°C
@Thickness 3.20 mm
183
°F
@Thickness 0.126 in
unannealed; ASTM D648
99.0
°C
@Thickness 6.40 mm
210
°F
@Thickness 0.252 in
unannealed; ASTM D648
Vicat Softening Point
120
°C
248
°F
Rate B/50; ISO 306
122
°C
252
°F
Rate B/50; ASTM D1525
125
°C
257
°F
Rate B/120; ISO 306
UL RTI, Electrical
75.0
°C
167
°F
UL 746B
UL RTI, Mechanical with Impact
75.0
°C
167
°F
UL 746B
UL RTI, Mechanical without Impact
75.0
°C
167
°F
UL 746B
Flammability, UL94
HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
UL 94
Processing Properties
Metric
English
Comments
Nozzle Temperature
255
-
270
°C
491
-
518
°F
Injection Molding
Zone 1
170
-
205
°C
338
-
401
°F
Sheet Extrusion
245
-
265
°C
473
-
509
°F
Zone 2
195
-
255
°C
383
-
491
°F
Sheet Extrusion
250
-
270
°C
482
-
518
°F
Zone 3
205
-
280
°C
401
-
536
°F
Sheet Extrusion
255
-
275
°C
491
-
527
°F
Zone 4
205
-
280
°C
401
-
536
°F
Sheet Extrusion
Adapter Temperature
225
-
280
°C
437
-
536
°F
Sheet Extrusion
Die Temperature
230
-
280
°C
446
-
536
°F
Sheet Extrusion
Melt Temperature
245
-
275
°C
473
-
527
°F
260
-
275
°C
500
-
527
°F
Mold Temperature
65.0
-
90.0
°C
149
-
194
°F
Roll Temperature
70.0
-
80.0
°C
158
-
176
°F
Roll Stack Temp - Top
75.0
-
80.0
°C
167
-
176
°F
Roll Stack Temp - Middle
80.0
-
95.0
°C
176
-
203
°F
Roll Stack Temp - Bottom
Drying Temperature
110
°C
230
°F
Injection Molding
110
-
115
°C
230
-
239
°F
Sheet Extrusion
Dry Time
4.00
-
6.00
hour
4.00
-
6.00
hour
Injection Molding
4.00
-
6.00
hour
4.00
-
6.00
hour
Sheet Extrusion
8.00
hour
8.00
hour
Cumulative; Injection Molding
8.00
hour
8.00
hour
Cumulative; Sheet Extrusion
Moisture Content
0.00 - 0.020 %
0.00 - 0.020 %
0.020 %
0.020 %
Back Pressure
0.300
-
0.700
MPa
43.5
-
102
psi
Shot Size
50 - 80 %
50 - 80 %
Vent Depth
0.00130
-
0.00200
cm
0.000512
-
0.000787
in
Screw Speed
50
-
80
rpm
50
-
80
rpm
Descriptive Properties
UV-light, water exposure/immersion
F2
UL 746C
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABI10822 / 244289
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.