MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Sandvik Kanthal Super RA Molybdenum disilicide
Categories: Metal; Ferrous Metal

Material Notes: Kanthal Super RA is specially designed to work in nitrogen at temperatures above 1250°C (2280°F). Other Kanthal Super elements have an excellent lifetime in oxidizing atmospheres but when operating in nitrogen, nitration occurs. At temperatures above 1250°C (2280°F), the protective glaze is consumed and the silicon in the silicide of the elements may react with nitrogen forming silicon nitride, which can cause scaling. The speed of the process depends on the dew point and the time in the atmosphere. The solution to these problems has been to run the elements in the air at high temperature for a couple of hours to restore the glaze. Kanthal Super RA withstands nitration at high temperatures better than any other type of Kanthal Super element. The nitration process still occurs, but to a 50% lower rate than for Kanthal Super 1800. The temperature, at which the weight reduction starts, is about 75°C (167°F) higher. The element has also substantially longer lifetime on all reducing and oxygen deficient atmospheres and possesses a higher tolerance to other aggressive environments

Special features:

  • Longer life at high temperatures in reactive atmospheres
  • Long life in all reducing and oxygen deficient atmospheres
  • Can be used in nitrogen up to 1700°C (3090°F) at a 40°C (104°F) dew point
  • Standard and specially designed elements
Typical applications for Kanthal Super RA are with different types of sintering, forging and heat treatment furnaces.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 5.60 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 75.0 - 125 MPa
@Temperature 1500 °C
Elongation at Break 9.0 %
Flexural Strength 350 - 400 MPa
Compressive Strength 1400 - 1500 MPa
Fracture Toughness 3.00 - 4.00 MPa-m½
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.00 - 8.00 µm/m-°C
Specific Heat Capacity 0.420 J/g-°C
Thermal Conductivity 15.0 W/m-K
@Temperature 600 - 1200 °C
 30.0 W/m-K
@Temperature 20.0 - 600 °C
Maximum Service Temperature, Air 1700 °C
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.70 - 0.80

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Molybdenum Disilicide, MoSi2
Vitreous Carbon (Glassy Carbon)
Rhenium, Re; Annealed
Pyrolytic Graphite, Low Temperature Isotropic (LTI)
PSM Industries Pacific Sintered Metals FCC-200-P High Carbon Copper Steel Powdered Metal (MPIF FC-0505-40)

NSANDV5033 / 199597

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.