Physical Properties | Original Value | Comments |
---|
Specific Gravity | 2.82 g/cc |
|
Chemical Properties | Original Value | Comments |
---|
Acid Class, SR | 52.2 |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 630 @Load 0.0999 kg |
Modulus of Elasticity | 100.8 GPa |
Modulus of Rigidity | 40.3 GPa |
Poissons Ratio | 0.252 |
Abrasion | 100 |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 6.60 µm/m-°C @Temperature -30.0 - 70.0 °C |
| 8.10 µm/m-°C @Temperature 100 - 300 °C |
Thermal Conductivity | 1.126 W/m-K @Temperature 35.0 °C |
Transformation Temperature, Tg | 527 °C |
Softening Point | 619 °C |
Annealing Point | 520 °C |
Strain Point | 489 °C |
|
Optical Properties | Original Value | Comments |
---|
Refractive Index | 1.56051 @Wavelength 2325.42 nm |
| 1.56687 @Wavelength 1970.09 nm |
| 1.57353 @Wavelength 1529.58 nm |
| 1.57908 @Wavelength 1128.64 nm |
| 1.58082 @Wavelength 1013.98 nm |
| 1.58373 @Wavelength 852.11 nm |
| 1.58566 @Wavelength 768.19 nm |
| 1.5874 @Wavelength 706.52 nm |
| 1.58911 @Wavelength 656.27 nm |
| 1.58958 @Wavelength 643.85 nm |
| 1.59002 @Wavelength 632.8 nm |
| 1.59199 @Wavelength 589.29 nm |
| 1.59208 @Wavelength 587.56 nm |
| 1.5944 @Wavelength 546.07 nm |
| 1.59881 @Wavelength 486.13 nm |
| 1.59936 @Wavelength 479.99 nm |
| 1.60335 @Wavelength 441.57 nm |
| 1.60404 @Wavelength 435.835 nm |
| 1.60836 @Wavelength 404.656 nm |
| 1.6157 @Wavelength 365.015 nm |
Abbe Number | 60.77 |
| 61 |
Optical Dispersion | 0.002974 |
| 0.003444 |
| 0.004322 |
| 0.004815 |
| 0.004966 |
| 0.005224 |
| 0.00529 |
| 0.008288 |
| 0.008763 |
| 0.009707 |
| 0.009781 |
| 0.01166 |
| 0.011957 |
| 0.016335 |
Transmission, Visible | 98.4 % @Thickness 10.0 mm, Wavelength 380 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 390 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 400 nm |
| 99.3 % @Thickness 10.0 mm, Wavelength 420 nm |
| 99.3 % @Thickness 10.0 mm, Wavelength 440 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 460 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 480 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 500 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 600 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 650 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 700 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 550 nm |
IR Transmittance | 81 % @Thickness 10.0 mm, Wavelength 2400 nm |
| 93.4 % @Thickness 10.0 mm, Wavelength 2200 nm |
| 97.8 % @Thickness 10.0 mm, Wavelength 2000 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 1800 nm |
| 99.1 % @Thickness 10.0 mm, Wavelength 1400 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 1600 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 1000 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 1200 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 900 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 800 nm |
UV Transmittance | 6.0 % @Thickness 10.0 mm, Wavelength 300 nm |
| 27 % @Thickness 10.0 mm, Wavelength 310 nm |
| 53 % @Thickness 10.0 mm, Wavelength 320 nm |
| 73 % @Thickness 10.0 mm, Wavelength 330 nm |
| 85 % @Thickness 10.0 mm, Wavelength 340 nm |
| 92.2 % @Thickness 10.0 mm, Wavelength 350 nm |
| 95.6 % @Thickness 10.0 mm, Wavelength 360 nm |
| 97.5 % @Thickness 10.0 mm, Wavelength 370 nm |
|
Descriptive Properties |
---|
Acid Resistance, Powder Method, RA(P) | 4 |
CCI | 0.00 B |
| 0.23 G |
| 0.23 R |
coloring, λ 5 | 295 |
coloring, λ 80 | 345 |
Coloring, Internal Transmission λ 0.05 | 300 |
Coloring, Internal Transmission λ 0.80 | 336 |
Knoop Hardness Class | 6 |
Ohara Code d | 592610 |
Ohara Code e | 594608 |
Phosphate Resistance, PR | 3.2 |
Photoelastic Constant (ß) | 2.29 |
Water Resistance, RW(P) | 2 |
Weathering Resistance (Surface Method) W(S)max | 3 |
Yield Point, At (°C) | 567 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.