MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Eastman Eastobond™ Renew 19412-100 Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Eastman Eastobond™ Renew copolyester 19412-100 is a plastic lidding film resin designed to adhere directly to monolayer PET food trays, rendering them recyclable. With Eastobond™ Renew, packaging converters can eliminate the polyolefin lining in their PET trays, reducing cost and making the end product recyclable. Eastobond™ Renew enables fast-moving consumer goods brand owners to achieve recyclable trays and reduce their consumption of fossil-based resources without sacrificing aesthetics or quality. Eastman Renew polymers have been certified by International Sustainability & Carbon Certification (ISCC), a global, independent agency for tracking sustainable content in a variety of industries. Renew polymers are produced with ISCC certified circular content by mass balance allocation.

Applications

  • Multi-layer film food contact
Key Attributes
  • BPA Free
  • Cost savings from eliminating tray liner
  • Does not require additional adhesives
  • Enables food tray recyclability
  • Excellent adhesion to monolayer PET
  • Not a material of concern
  • Polyolefin replacement

Information provided by Eastman.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.715 g/cc0.0258 lb/in³ASTM D1895
Density 1.31 g/cc0.0473 lb/in³ASTM D1505
 1.33 g/cc0.0480 lb/in³Crystalline; ASTM D1505
 1.20 g/cc
@Temperature 250 °C
0.0434 lb/in³
@Temperature 482 °F
Note A- Table 2; D 1238
Water Vapor Transmission 39.0 g/m²/day2.51 g/100 in²/dayASTM F372
Oxygen Transmission 3.10 cc-mm/m²-24hr-atm7.87 cc-mil/100 in²-24hr-atmASTM D3985
Carbon Dioxide Transmission 16.7 cc-mm/m²-24hr-atm42.4 cc-mil/100 in²-24hr-atm
Viscosity Measurement 0.6500.650Inherent, film, EMN-A-AC-G-V-1
 0.7400.740Inherent, EMN-A-AC-G-V-1
Thickness 50.0 microns1.97 mil
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 45.0 MPa6530 psiASTM D882
Elongation at Break <= 5.00 %<= 5.00 %ASTM D882
Tensile Modulus 2.20 GPa319 ksiASTM D882
Tear Strength, Total 0.300 N0.0674 lb (f)Elmendorf; ASTM D1922
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity  1.15 J/g-°C
@Temperature 25.0 °C
0.275 BTU/lb-°F
@Temperature 77.0 °F
DSC
 1.60 J/g-°C
@Temperature 75.0 °C
0.382 BTU/lb-°F
@Temperature 167 °F
DSC
 1.80 J/g-°C
@Temperature 125 °C
0.430 BTU/lb-°F
@Temperature 257 °F
DSC
 2.00 J/g-°C
@Temperature 200 °C
0.478 BTU/lb-°F
@Temperature 392 °F
DSC
 2.10 J/g-°C
@Temperature 250 °C
0.502 BTU/lb-°F
@Temperature 482 °F
DSC
 2.15 J/g-°C
@Temperature 290 °C
0.514 BTU/lb-°F
@Temperature 554 °F
DSC
Thermal Conductivity 0.210 W/m-K1.46 BTU-in/hr-ft²-°FASTM C177
Glass Transition Temp, Tg 51.0 °C124 °FASTM D3418
 
Optical PropertiesMetricEnglishComments
Haze <= 0.500 %<= 0.500 %ASTM D1003
Gloss 95.0 %95.0 %ASTM D2457
Transmission, Visible 90.0 %90.0 %Regular; ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEATM4134 / 323757

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.