(Viewing data as-entered.
Click here
to return)
Chevron Phillips Marlex® C513UV HDPE Blow Molding Resin
Categories:
Polymer
;
Thermoplastic
;
Polyethylene (PE)
;
High Density (HDPE)
;
High Density Polyethylene (HDPE), Blow Molding Grade
Material Notes:
Resin Type:
Hexene Copolymer
Characteristics:
Outstanding impact resistance
Excellent ESCR
Excellent processability
UV stabilization
Applications:
Intermediate bulk containers
Agricultural containers
Information provided by Chevron Phillips.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
0.945
g/cc
ASTM D1505
ESCR 100% Igepal®
>=
2000
hour
Conditions A and B; ASTM D1693
Melt Flow
6.2
g/10 min
Condition 190/2.16, HLMI; ASTM D1238
Mechanical Properties
Original Value
Comments
Hardness, Shore D
61
ASTM D2240
Tensile Strength, Yield
24.0
MPa
2 in/min, Type IV bar; ASTM D638
Elongation at Break
700 %
2 in/min, Type IV bar; ASTM D638
Flexural Modulus
1.07
GPa
Tangent, 16:1 span:depth,0.5in/min; ASTM D790
Tensile Impact Strength
580
kJ/m²
Type S bar; ASTM D1822
Thermal Properties
Original Value
Comments
Deflection Temperature at 0.46 MPa (66 psi)
66.0
°C
Method A; ASTM D648
Vicat Softening Point
123
°C
Loading 1, Rate A; ASTM D1525
Brittleness Temperature
<=
-75.0
°C
Type A, type 1 specimen; ASTM D746
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Borealis Borstar® FB3450 HDPE for Film Extrusion
Borealis Bormed™ HE2581-PH HDPE for Healthcare Applications
Equate EMDA-6147 HDPE Blow Molding Resin
Formosa Plastics Formolene® HB5502Z Blow Molding HDPE
Global B-5200 High Density Polyethylene
PCHEVD016 / 20634
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.