MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPV 4180 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 4100 series are engineered materials designed primarily for demanding automotive and industrial applications. Available in both black and natural, this product is a low density, higher hardness thermoplastic vulcanizate featuring excellent flex fatigue resistance, compression set, heat aging and resilience to be used in injection molded parts, extruded profiles, hose and tubing. It can be blow molded into boots ducts and other articles.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Fatigue Resistant; Good Adhesion; Good Melt Strength; Good Moldability; Good Processability; Good Surface Finish; Heat Aging Resistant; High Hardness; High Melt Stability; Low Density; Low Specific Gravity; Medium Heat Resistant; Resilient

Uses: Agricultural Applications; Appliance Components; Automotive Applications; Automotive Exterior Parts; Automotive Interior Parts; Automotive Under the Hood; Blow Molding Applications; Hose; Industrial Applications; Plugs; Profiles; Rubber Replacement; Tubing; White Goods & Small Appliance

Agency Ratings: UL 94

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER MS-AR-100 DGN Color: Black; CHRYSLER MS-AR-100 DGN Color: Natural; FORD WSD-M2D381-A1 Color: Black; FORD WSD-M2D381-A1 Color: Natural; GM GMP.E/P.004 Color: Black; GM GMP.E/P.004 Color: Natural; GM GMW/15813 Type 7 Color: Black; GM GMW/15813 Type 7 Color: Natural; GM QK 3525 Type 5 Color: Black; GM QK 3525 Type 5 Color: Natural

UL File Number: QMFZ2. E54709

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.960 g/ccISO 1183
Viscosity 340 cP
@Shear Rate 206 1/s,
Temperature 200 °C
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 79
@Time 5.00 sec
Extruded; ASTM D2240
 83
@Time 5.00 sec
Injection Molded; ASTM D2240
Tensile Strength 1310 psiFlow; ISO 37
 1480 psiAcross Flow; ISO 37
 1330 psi
@Thickness 4270 mm,
Temperature 150 °C
Across Flow, Change in Air; ISO 188
 1350 psi
@Thickness 25400 mm,
Temperature 135 °C
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain 653 psi
@Strain 100 %
Across Flow; ISO 37
 986 psi
@Strain 100 %
Flow; ISO 37
 686 psi
@Strain 100 %,
Treatment Temp. 150 °C
Across Flow, Change in Air at 168 hr; ISO 188
 718 psi
@Strain 100 %,
Treatment Temp. 135 °C
Across Flow, Change in Air at 1000 hr; ISO 188
Elongation at Break 330 %Flow; ASTM D412
 620 %Across Flow; ASTM D412
 527 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
Across Flow, Change in Air; ISO 188
 527 %
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air; ISO 188
Tear Strength 270 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set 26 %
@Temperature 22.8 °C,
Time 79200 sec
ISO 815
 40 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 58 %
@Temperature 125 °C,
Time 252000 sec
ISO 815
 
Thermal PropertiesOriginal ValueComments
UL RTI, Electrical 212 °FUL 746
UL RTI, Mechanical with Impact 149 °FUL 746
UL RTI, Mechanical without Impact 212 °FUL 746
Flammability, UL94 HB
@Thickness 1.02 mm
All Colors
 
Processing PropertiesOriginal ValueComments
Processing Temperature 369 - 428 °FInjection
Rear Barrel Temperature 356 - 419 °FInjection
Middle Barrel Temperature 356 - 419 °FInjection
Front Barrel Temperature 356 - 419 °FInjection
Nozzle Temperature 369 - 428 °FInjection
Zone 1 356 - 392 °FExtrusion
Zone 2 356 - 401 °FExtrusion
Zone 3 369 - 410 °FExtrusion
Zone 4 369 - 410 °FExtrusion
Die Temperature 383 - 419 °FExtrusion
Melt Temperature 383 - 419 °FExtrusion
Mold Temperature 50.0 - 131 °FInjection
Drying Temperature 180 °F
Dry Time 3.00 hour
Screw Speed 100 - 200 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ1160 / 237651

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.