MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

(Viewing data as-entered. Click here to return)
Avient Gravi-Tech™ GRV-NP-110-W-NAT Polyamide 12 (Nylon 12)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes:

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 11.0 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 27.2 MPaType I, 5.1 mm/min; ASTM D638
Elongation at Break 1.8 %Type I, 5.1 mm/min; ASTM D638
Tensile Modulus 8270 MPaType I, 5.1 mm/min; ASTM D638
Flexural Strength 48.3 MPaASTM D790
Flexural Modulus 4960 MPaASTM D790
Poissons Ratio 0.35ASTM E132
Shear Modulus 3.06 GPaCalculated
Izod Impact, Notched 110 J/m
@Thickness 3.18 mm,
Temperature 23.0 °C
Injection Molded; ASTM D256A
Izod Impact, Unnotched 370 J/m
@Thickness 3.18 mm,
Temperature 23.0 °C
Injection Molded; ASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 63.0 µm/m-°C
@Temperature 0.000 - 32.0 °C
ASTM E831
 100 µm/m-°C
@Temperature 60.0 - 100 °C
ASTM E831
CTE, linear, Transverse to Flow 57.0 µm/m-°C
@Temperature 0.000 - 32.0 °C
ASTM E831
 84.0 µm/m-°C
@Temperature 60.0 - 100 °C
ASTM E831
Thermal Conductivity 3.50 W/m-KThe value listed as thermal conductivity, ASTM C177, was tested in accordance with ASTM E1461.; ASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 138 °C
@Thickness 6.35 mm
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 87.8 °C
@Thickness 6.35 mm
Unannealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 - 288 °C
Mold Temperature 82.2 - 149 °C
Drying Temperature 79.4 °C
Dry Time 4.00 hour
 
Descriptive Properties
AdditiveImpact Modifier
AppearanceNatural Color
FeaturesHigh Density
 Impact Modified
 Non-Toxic
FormsPellets
Generic MaterialNylon 12
Generic NamePolyamide 12 (Nylon 12)
Processing MethodInjection Molding
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
UsesIndustrial Applications
 Medical/Healthcare Applications
 Projectiles
 Radiation Shielding
 Sporting Goods
 Weighting & Balancing

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Techmer ES HiFill® PA6 1030
Techmer ES HiFill® PA6 1020
Techmer ES HiFill® TPU 1000
Evonik VESTOSINT® 1101 white Polyamide 12
Evonik VESTAMID® LX9012 PA 12

PH0POL0687 / 145256

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.