MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Teknor Apex Chemlon® 66A 9516 Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, MoS2 Filled

Material Notes: Notes: 66A 9516 is an injection molding grade of nylon 66 containing molybdenum disulphide to reduce the coefficient of friction and improve wear resistance. It is well suited to applications involving moving parts such as bearings bushes, gear wheels, etc.

Availability: Europe

Additive: Molybdenum Disulfide Lubricant

Features: Low Friction; Lubricated; Wear Resistant

Uses: Bearings; Bushings; Gears

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.15 g/cc0.0415 lb/in³ISO 1183
Moisture Absorption at Equilibrium 2.5 %2.5 %50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.014 - 0.019 cm/cm0.014 - 0.019 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 75.2 MPa10900 psiISO 527-2
Tensile Modulus 3.00 GPa435 ksiISO 527-2
Flexural Strength 75.2 MPa10900 psiISO 178
Flexural Modulus 2.70 GPa392 ksiISO 178
Izod Impact, Notched (ISO) 5.04 kJ/m²2.40 ft-lb/in²ISO 180/A
Izod Impact, Unnotched (ISO) 35.7 kJ/m²17.0 ft-lb/in²ISO 180
Charpy Impact Unnotched NBNBISO 179/1eU
Charpy Impact, Notched 0.903 J/cm²4.30 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmIEC 60093
Surface Resistance 1.00e+14 ohm1.00e+14 ohmIEC 60093
Dielectric Strength 16.9 kV/mm
@Thickness 3.00 mm
430 kV/in
@Thickness 0.118 in
IEC 60243-1
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 190 °C374 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 75.0 °C167 °FUnannealed; ISO 75-2/A
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0600 in
Oxygen Index 24 %24 %ISO 4589-2
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 270 - 290 °C518 - 554 °F
Middle Barrel Temperature 270 - 290 °C518 - 554 °F
Front Barrel Temperature 270 - 290 °C518 - 554 °F
Melt Temperature 270 - 290 °C518 - 554 °F
Mold Temperature 80.0 - 90.0 °C176 - 194 °F
Drying Temperature 80.0 °C176 °F
Dry Time 2.00 hour2.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ0399 / 236890

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.