MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Covestro Desmopan® DP 1485A Polyurethane  (discontinued **)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Extrusion- and injection molding grade; suitable for extrusion blow molding; very large processing window; high melt stability; Beads; Application; Bellows; Hoses, non-reinforced; Profiles; Injection molded engineering parts

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.22 g/cc0.0440 lb/in³ISO 1183
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8484ISO 868
Hardness, Shore D 3333ISO 868
Tensile Strength, Ultimate 45.0 MPa6530 psiDIN 53504; DIN 53504
Tensile Stress at Strain  5.20 MPa
@Strain 100 %
754 psi
@Strain 100 %
DIN 53504; DIN 53504
 9.00 MPa
@Strain 300 %
1310 psi
@Strain 300 %
DIN 53504; DIN 53504
Elongation at Break 695 %695 %200 mm/min; DIN 53504
Tensile Modulus  0.0210 GPa
@Temperature 60.0 °C
3.05 ksi
@Temperature 140 °F
storage; ISO 6721-1,-4
 0.0310 GPa
@Temperature 20.0 °C
4.50 ksi
@Temperature 68.0 °F
storage; ISO 6721-1,-4
 0.290 GPa
@Temperature -20.0 °C
42.1 ksi
@Temperature -4.00 °F
storage; ISO 6721-1,-4
Rebound 44 %44 %Resilience; ISO 4662
Tear Strength 63.0 kN/m359 pli500 mm/min; ISO 34-1
Abrasion 3030mm³, Method A; ISO 4649
Compression Set  19 %
@Temperature 23.0 °C
19 %
@Temperature 73.4 °F
72 hr; ISO 815
 40 %
@Temperature 70.0 °C
40 %
@Temperature 158 °F
24; ISO 815
 29 %
@Temperature 70.0 °C,
Time 86400 sec
29 %
@Temperature 158 °F,
Time 24.0 hour
Method C; ISO 815-1
 
Processing PropertiesMetricEnglishComments
Melt Temperature 200 - 220 °C392 - 428 °FExtrusion
 200 - 240 °C392 - 464 °FInjection
Mold Temperature 20.0 °C68.0 °FInjection
Drying Temperature 80.0 °C176 °F

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Desmopan® 1080A Polyurethane
Covestro Desmopan® 3385A Polyurethane
Covestro Desmopan® 2586A Polyurethane
Covestro Desmopan® 588 E Polyurethane
Covestro Desmopan® DP 1490A Polyurethane

PB09775 / 92615

Polyurethane

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.