MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Oxygen-free silver-bearing Copper, UNS C10500
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent hot and cold workability; good forgeability. Fabricated by coining, coppersmithing, drawing and upsetting, hot forging and pressing, spinning, swaging, stamping.

Applications: auto gaskets, radiators, busbars, conductivity wire, contacts, radio parts, winding, switches, terminals, commutator segments, chemical process equipment, printing rolls, clad metals, printed circuit foil.

Available as flat products, rod, wire, tube and shapes. Similar alloys distinguished only by silver content: 8 oz/ton Ag (UNS C10400), 10 oz/ton Ag (UNS C10500), 25 oz/ton Ag (UNS C10700).

Key Words: AMSIL Copper; Oxygen-free Silver-Copper
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.94 g/ccUNS C10700
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 221 - 455 MPa
 70.0 MPa
@Temperature 450 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 70.0 MPa
@Temperature 450 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 70.0 MPa
@Temperature 450 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 70.0 MPa
@Temperature 450 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 75.0 MPa
@Temperature 400 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 75.0 MPa
@Temperature 350 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 75.0 MPa
@Temperature 415 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 75.0 MPa
@Temperature 440 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 100 MPa
@Temperature 420 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 100 MPa
@Temperature 400 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 100 MPa
@Temperature 375 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 100 MPa
@Temperature 320 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 150 MPa
@Temperature 295 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 150 MPa
@Temperature 360 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 150 MPa
@Temperature 275 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 150 MPa
@Temperature 400 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 200 MPa
@Temperature 390 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 200 MPa
@Temperature 285 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 200 MPa
@Temperature 370 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 200 MPa
@Temperature 350 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 300 MPa
@Temperature 360 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 300 MPa
@Temperature 335 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 300 MPa
@Temperature 380 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 300 MPa
@Temperature 270 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 350 MPa
@Temperature 260 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 350 MPa
@Temperature 375 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 350 MPa
@Temperature 325 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 350 MPa
@Temperature 350 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 400 MPa
@Temperature 320 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 400 MPa
@Temperature 345 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 400 MPa
@Temperature 225 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 400 MPa
@Temperature 290 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 410 MPa
@Temperature 200 °C
0.044 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 410 MPa
@Temperature 200 °C
silver free; wire cold worked 90% to a diameter of 2 mm and then annealed 1/2 h at various temperatures
 410 MPa
@Temperature 200 °C
0.114 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
 410 MPa
@Temperature 200 °C
0.085 Ag; wire cold worked 90% to a diameter of 2mm and then annealed 1/2 h at various temperatures
Tensile Strength, Yield 69.0 - 365 MPaDepending on temper
Elongation at Break 55 %in 101.6 mm (4 in.)
Modulus of Elasticity 115 GPa
Poissons Ratio 0.30Calculated
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 65 %
Shear Modulus 44.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000172 ohm-cm100% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.0 µm/m-°C
@Temperature 20.0 - 100 °C
 17.3 µm/m-°C
@Temperature 20.0 - 200 °C
 17.7 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0920 BTU/lb-°F
Thermal Conductivity 388 W/m-K
@Temperature 20.0 °C
Melting Point 1083 °C
Solidus 1083 °C
Annealing Point >= 900 °F
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu >= 99.95 %Includes Ag
Silver, Ag >= 0.034 %Min 10 troy oz./ton

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Oxygen-free electronic Copper, UNS C10100
Oxygen-free high conductivity Copper, Hard, UNS C10200
Oxygen-free high conductivity Copper, Soft, UNS C10200
Oxygen-free silver-bearing Copper, UNS C10700
Overview of materials for Copper Alloy

MC10500d2 / 10471

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.