MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Chosun Refractories RGM-20 Blast Furnace Runner Refractory
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes:

Information provided by Chosun Refractories via Korea Institute of Ceramic Engineering and Technology (KICET).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density  2.40 g/cc
@Temperature 1450 °C,
Time 7200 sec
0.0867 lb/in³
@Temperature 2640 °F,
Time 2.00 hour
 2.50 g/cc
@Temperature 110 °C,
Time 86400 sec
0.0903 lb/in³
@Temperature 230 °F,
Time 24.0 hour
Porosity  24.3 %
@Temperature 110 °C,
Time 86400 sec
24.3 %
@Temperature 230 °F,
Time 24.0 hour
 27.2 %
@Temperature 1450 °C,
Time 7200 sec
27.2 %
@Temperature 2640 °F,
Time 2.00 hour
 
Mechanical PropertiesMetricEnglishComments
Modulus of Rupture  0.0074556 GPa
@Temperature 110 °C,
Time 86400 sec
1.0814 ksi
@Temperature 230 °F,
Time 24.0 hour
 0.00981 GPa
@Temperature 1450 °C,
Time 10800 sec
1.42 ksi
@Temperature 2640 °F,
Time 3.00 hour
Compressive Strength  13.6 MPa
@Treatment Temp. 110 °C,
Time 86400 sec
1980 psi
@Treatment Temp. 230 °F,
Time 24.0 hour
Cold Crushing Strength
 28.7 MPa
@Treatment Temp. 1450 °C,
Time 7200 sec
4170 psi
@Treatment Temp. 2640 °F,
Time 2.00 hour
Cold Crushing Strength
 
Thermal PropertiesMetricEnglishComments
Shrinkage -0.220 %
@Temperature 1450 °C,
Time 7200 sec
-0.220 %
@Temperature 2640 °F,
Time 2.00 hour
 
Component Elements PropertiesMetricEnglishComments
Al2O3 64 %64 %
SiC 16 %16 %
 
Descriptive Properties
Installation MethodSpray
Main ApplicationsMain runner Gunning Material
Material Required for Estimating (kg/m3)2,500

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CCHOS277 / 124221

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.