MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Toyobo GLAMIDE® TY-791GT 6T-Nylon
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon, Aromatic

Material Notes: GLAMIDE® is very tough and exhibits high abrasion resistance. It has a high melting point and heat resistance, has well-balanced proportions of mechanical properties, performs self-distinguishing and a specific grade approved as UL94V-0 class is provided, and it exhibits excellent chemical resistance and oil resistance. Grade TY-791GT is a GF reinforced, aromatic 6T-Nylon. It has a good finish of coating and contains 55% GF.

55

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.64 g/ccAbsolute Drying; ASTM-D792
Filler Content 55 %
Water Absorption 0.80 %Absolute Drying; ASTM-D570
Moisture Absorption at Equilibrium 1.0 %Absolute Drying; ASTM-D570
Linear Mold Shrinkage 0.0010 - 0.0020 cm/cm
@Thickness 1.00 mm
Absolute Drying
 0.0020 - 0.0050 cm/cm
@Thickness 3.00 mm
Absolute Drying
Melt Flow 10 g/10 min
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 120Absolute Drying; ASTM-D785
Tensile Strength, Ultimate 105 MPa
@Temperature 80.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D638
 120 MPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D638
 165 MPa
@Temperature 23.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D638
 230 MPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D638
 250 MPa
@Temperature -40.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D638
 280 MPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D638
Elongation at Break 1.6 %Absolute Drying; ASTM-D638
 2.0 %Practical Use (Water Absorption 1.0%); ASTM-D638
Flexural Strength 160 MPa
@Temperature 80.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D790
 180 MPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D790
 280 MPa
@Temperature 23.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D790
 320 MPa
@Temperature -40.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D790
 320 MPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D790
 355 MPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D790
Flexural Modulus 5.00 GPa
@Temperature 80.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D790
 7.50 GPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D790
 13.0 GPa
@Temperature 23.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D790
 15.0 GPa
@Temperature -40.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D790
 16.0 GPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D790
 16.5 GPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D790
Compressive Strength 150 MPaAbsolute Drying; ASTM-D695
Izod Impact, Notched 70.0 J/m
@Temperature -40.0 °C
Absolute Drying; ASTM-D256
 85.0 J/m
@Temperature -40.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D256
 143 J/m
@Temperature 23.0 °C
Absolute Drying; ASTM-D256
 180 J/m
@Temperature 23.0 °C
Practical Use (Water Absorption 1.0%); ASTM-D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+12 ohm-cmAbsolute Drying; ASTM-D257
Dielectric Strength 21.0 kV/mm
@Thickness 2.00 mm
Practical Use (Water Absorption 1.0%); ASTM-D149
 28.0 kV/mm
@Thickness 2.00 mm
Absolute Drying; ASTM-D149
Arc Resistance 94 secPractical Use (Water Absorption 1.0%); ASTM-D495
 100 secAbsolute Drying; ASTM-D495
Comparative Tracking Index 550 VIEC Method
 
Thermal PropertiesOriginal ValueComments
CTE, linear 19.0 µm/m-°CAbsolute Drying; ASTM-D696
Deflection Temperature at 0.46 MPa (66 psi) 217 °CAbsolute Drying; ASTM-D648
Deflection Temperature at 1.8 MPa (264 psi) 217 °CAbsolute Drying; ASTM-D648
Flammability, UL94 HB
 
Processing PropertiesOriginal ValueComments
Melt Temperature 270 - 290 °C
Mold Temperature 80.0 - 100 °C
Injection Pressure 30.0 - 70.0 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Toyobo GLAMIDE® TY-592GHV 6T-Nylon
Toyobo GLAMIDE® TY-502NZ 6T-Nylon
Toyobo GLAMIDE® TY-791HT 6T-Nylon
Toyobo GLAMIDE® T-808-02 Nylon-6
Toyobo GLAMIDE® T-402FR Nylon-6

PTOY937 / 107488

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.