MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EMS-Grivory Grilamid® LC-15H black PA12-CF15
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12); Nylon 12, Carbon Fiber Filled

Material Notes: Product description: Grilamid LC-15H black is a Polyamide 12 injection molding product reinforced with 15% carbon fibers. The product is inherently black and is only available in this color.

Main Attributes:

  • high stiffness at low weight
  • very low moisture absorption
  • electrically conductive
  • favorable abrasion and wear properties
  • low coefficient of thermal expansion
  • low mould shrinkage
  • easy processing
  • good chemical and UV resistance
Grilamd LC-15H black is particularly suitable for technical components in the following application fields:
  • Sport and leisure goods
  • Lightweight designs and prototypes
  • Tools and instruments
  • Conductive electrical devices
  • Explosion proof safety devices

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.07 g/ccDry; ISO 1183
Water Absorption 1.1 %Sim. to ISO 62
Moisture Absorption 0.700 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0050 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 100 MPaConditioned; ISO 2039-1
Tensile Strength at Break 100 MPaConditioned; ISO 527-1/-2
 110 MPaDry; ISO 527-1/-2
Elongation at Break 4.5 %Dry; ISO 527-1/-2
 5.0 %Conditioned; ISO 527-1/-2
Tensile Modulus 7500 MPaConditioned; ISO 527-1/-2
 9500 MPaDry; ISO 527-1/-2
Charpy Impact Unnotched 40.0 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eU
 40.0 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eA
 10.0 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 100 ohm-cmConditioned; IEC 60093
Surface Resistance 50 ohmIEC 60093
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 10.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 150 µm/m-°CISO 11359-1/-2
Melting Point 178 °C10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 90.0 - 120 °CLong Term; ISO 2578
 150 °CShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 160 °CISO 75-1/-2
Deflection Temperature at 8.0 MPa 100 °CISO 75-1/-2
Flammability, UL94 HBIEC 60695-11-10
 
Descriptive Properties
Electricals & ElectronicsMobile phones and other portable devices
FormGranules
Industry & Consumer goodsMechanical Engineering
 Medical devices
 Power transmission
 Sports & Leisure
 Tools & Accessories
ProcessingInjection Molding
Special CharacteristicsAnti-static
 High impact or impact modified
 Improved UV resistance (outdoor use)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
EMS-Grivory Grilamid® LV-15H nat PA12-GF15
EMS-Grivory Grilamid® LC-3H black PA12-CF30
EMS-Grivory Grilamid® LV-3H PA12-GF30
EMS-Grivory Grilamid® XE 3841 nat PA12
EMS-Grivory Grilamid® LV-23H PA12-GF23

PGRH065 / 156774

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.