MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zytel® FR7026V0F NC010 PA66-FR(30)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Unreinforced, Flame Retardant

Material Notes: Unreinforced, Flame Retardant, Non-Halogenated, Heat Stabilized, Polyamide 66

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.16 g/ccDAM; ISO 1183
Melt Density 1.03 g/cc
@Temperature 280 °C
Water Absorption 8.0 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
 1.8 %
@Thickness 2.00 mm,
Time 86400 sec
Immersion; DAM; Sim. to ISO 62
Moisture Absorption 2.50 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Viscosity Number 160 cm³/gDAM; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0090 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.010 cm/cmDAM; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 110 MPaH 358/30; DS; 50% RH; ISO 2039-1
Tensile Strength at Break 80.0 MPaDAM; ISO 527-1/-2
Tensile Strength, Yield 55.0 MPa50% RH; ISO 527-1/-2
Elongation at Break 10 %DAM; ISO 527-1/-2
 30 %Nominal; 50% RH; ISO 527-1/-2
Elongation at Yield 20 %50% RH; ISO 527-1/-2
Tensile Modulus 2000 MPa50% RH; ISO 527-1/-2
 3700 MPaDAM; ISO 527-1/-2
Poissons Ratio 0.36DAM
 0.4050% RH
Izod Impact, Notched (ISO) 4.40 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
Charpy Impact Unnotched 80.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
 110 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eU
Charpy Impact, Notched 2.00 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 3.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 3.50 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 7.00 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Surface Resistance >= 1.00e+15 ohm50% RH; IEC 62631-3-2
Dielectric Strength 31.0 kV/mmDAM; IEC 60243-1
Comparative Tracking Index 600 VDAM; IEC 60112
 >= 600 VPLC 0; DAM; UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 60.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 65.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ASTM E 831
 70.0 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
Specific Heat Capacity 2.59 J/g-°C
@Temperature 280 °C
Melt
Thermal Conductivity 0.170 W/m-K
@Temperature 280 °C
Melt
Melting Point 260 °C10°C/min; DAM; ISO 11357-1/-3
Hot Ball Pressure Test 220 °CDS; DAM; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 230 °CDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °CDAM; ISO 75-1/-2
Glass Transition Temp, Tg 20.0 °C10°C/min; 50% RH; ISO 11357-1/-2
 80.0 °C10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94 V-0
@Thickness 0.820 mm
DAM; IEC 60695-11-10
 V-0
@Thickness 1.50 mm
DAM; IEC 60695-11-10
Oxygen Index 39 %DAM; ISO 4589-1/-2
Glow Wire Ignition Temperature 960 °C
@Thickness 0.400 mm
DAM; IEC 60695-2-12
 960 °C
@Thickness 0.750 mm
DAM; IEC 60695-2-13
 960 °C
@Thickness 1.50 mm
DAM; IEC 60695-2-13
 960 °C
@Thickness 3.00 mm
DAM; IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.400 mm
DAM; IEC 60695-2-12
 960 °C
@Thickness 0.750 mm
DAM; IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
DAM; IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
DAM; IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 280 °COptimum, Injection
 270 - 290 °CRange, Injection
Mold Temperature 70.0 °COptimum, Injection
 50.0 - 90.0 °CInjection
Ejection Temperature 210 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Injection
Hold Pressure 50.0 - 100 MPaRange, Injection
 
Descriptive Properties
AdditivesFlame retardant
 Non-halogenated/Red phosphorous free flame retardant
 Release agent
Drying RecommendedyesInjection
FMVSS ClassDNIISO 3795 (FMVSS 302)
ISO designationISO 16396-PA66,FR(30),M1F1G1NR,S14-040
Max. screw tangential speed (m/s)0.2Injection
Odor Class5VDA 270
Part Marking Code>PA66-FR(30)<ISO 11469
PolymerPA66 FR(30)
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPA66-FR(30)ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Crastin® S650FR NC010 PBT-FR(17)
Celanese Zytel® FR7025V0F NC010 PA66-FR(30)
Celanese Zytel® 103HSL NC010 PA66
Celanese Minlon® 10B40 NC010 PA66-MD40
EMS-Grivory Grilamid® L 20 H FR PA12 FR

PDSX5422 / 198062

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.