MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Titanium Beta-CEZ ST 830°C (1525°F), Aged 550°C
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Near-beta alloy. High strength, high toughness, intermediate creep resistance. Good ductility and processing flexibility.

Applications: Heavy-section, forged compressor discs; as forged parts, springs and fasteners.

4 other heat treatments of this alloy are listed in MatWeb.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.69 g/cc
a Lattice Constant 2.9287 Åcph alpha phase
 3.204 Åbcc beta phase
c Lattice Constant 4.6606 Åcph alpha phase
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 1600 MPa
Tensile Strength, Yield 1520 MPa
Elongation at Break 2.0 %
Modulus of Elasticity 122 GPaUnaged
Tensile Modulus 100 GPa
@Temperature 400 °C
 106 GPa
@Temperature 300 °C
Poissons Ratio 0.33Typical for beta titanium alloy.
Shear Modulus 45.9 GPaCalculated from typical values.
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000150 ohm-cmEstimated from similar beta titanium alloys.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 8.20 µm/m-°C
@Temperature 20.0 °C
 9.60 µm/m-°C
@Temperature 250 °C
 11.3 µm/m-°C
@Temperature 500 °C
Specific Heat Capacity 0.508 J/g-°C
Thermal Conductivity 6.70 W/m-K
Melting Point 1550 - 1602 °C
Solidus 1550 °C
Liquidus 1602 °C
Beta Transus 890 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 5.0 %
Chromium, Cr 2.0 %
Iron, Fe 1.0 %
Molybdenum, Mo 4.0 %
Tin, Sn 2.0 %
Titanium, Ti 82 %
Zirconium, Zr 4.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Titanium Beta-CEZ ST 860°C (1580°F), Aged 550°C
Titanium Beta C (Ti-3Al-8V-6Cr-4Mo-4Zr ST 815°C, Aged 425°C
TIMET TIMETAL® 21S Titanium Alloy (Ti-15Mo-3Nb-3Al-0.2Si, ASTM Grade 21); 80% Cold Work
Titanium Ti-15Mo-5Zr ST 730°C, Aged 400°C
Titanium Ti-15Mo-5Zr-3Al Duplex Aged

MTBCE1 / 14211

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.