MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lubrizol Advanced Materials PEARLCOAT® DIPP-119 Thermoplastic Polyurethane Elastomer
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyether Grade

Material Notes: PEARLCOAT® DIPP-119 is polycaprolactone copolyester based thermoplastic polyurethane, supplied in form of translucent pellets. Featuring low melting point and excellent transparency, this product offers excellent flexibility, elasticity and easy processing. PEARLCOAT® DIPP-119 is used mostly in extrusion applications where low melting point as well as improved adhesion over polar substrates is highly appreciated. It is ideal for PVC compounding. It is also used in solvent coatings on textile substrates.

All information provided by Merquinsa

Key Words: TPU
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.16 g/cc1.16 g/ccASTM D792
Melt Flow 10 g/10 min
@Load 21.6 kg
10 g/10 min
@Load 47.6 lb
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7070ASTM D2240
Tensile Strength, Yield 20.04 MPa2906 psiASTM D412
Elongation at Break 750 %750 %ASTM D412
100% Modulus 3.00 MPa
@Strain 100 %
435 psi
@Strain 100 %
ASTM D412
300% Modulus 4.00 MPa
@Strain 300 %
580 psi
@Strain 300 %
ASTM D412
Tear Strength 50.1 kN/m286 pliASTM D624 (Die C)
Abrasion 4545loss (mm³); DIN 53.516
 
Thermal PropertiesMetricEnglishComments
Melting Point 118 - 128 °C244 - 262 °FMQSA 111
Glass Transition Temp, Tg -30.0 °C-22.0 °FDSC, 10ºC/min; DIN 51.007
 
Processing PropertiesMetricEnglishComments
Moisture Content <= 0.10 %<= 0.10 %MQSA 44

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Austin Novel Materials Texalan® 598A Polyether-based TPU
Austin Novel Materials Texalan® 698A Polyester and Polyether based TPU
Taiwan PU Corporation TPU-EH95 High Hydrolysis Resistance, Extrusion Molding Polyether Base TPU
Lubrizol Advanced Materials PEARLCOAT® 126K Thermoplastic Polyurethane Elastomer
Lubrizol Estane® 58123 Thermoplastic Polyurethane

PMES65 / 88442

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.