Physical Properties | Original Value | Comments |
---|
Density | 2.51 g/cc |
|
Chemical Properties | Original Value | Comments |
---|
Acid Class, SR | 1.0 |
Alkali Class, AR | 2.3 |
Stain Resistance Class, FR | 0.00 |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 610 |
Modulus of Elasticity | 82.0 GPa |
Poissons Ratio | 0.206 |
Shear Modulus | 34.0 GPa |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 7.10 µm/m-°C @Temperature -30.0 - 70.0 °C |
| 8.30 µm/m-°C @Temperature 20.0 - 300 °C |
Specific Heat Capacity | 0.858 J/g-°C |
Thermal Conductivity | 1.114 W/m-K |
Transformation Temperature, Tg | 557 °C |
Softening Point | 719 °C |
Annealing Point | 557 °C |
|
Optical Properties | Original Value | Comments |
---|
Refractive Index | 1.489 @Wavelength 2325.4 nm |
| 1.49495 @Wavelength 1970.1 nm |
| 1.50 @Wavelength 1529.6 nm |
| 1.506 @Wavelength 1060 nm |
| 1.507 @Wavelength 1014 nm |
| 1.509 @Wavelength 852.1 nm |
| 1.512 @Wavelength 706.5 nm |
| 1.514 @Wavelength 656.3 nm |
| 1.514 @Wavelength 643.8 nm |
| 1.515 @Wavelength 632.8 nm |
| 1.516 @Wavelength 587.6 nm |
| 1.516 @Wavelength 589.3 nm |
| 1.518 @Wavelength 546.1 nm |
| 1.522 @Wavelength 486.1 nm |
| 1.522 @Wavelength 480 nm |
| 1.526 @Wavelength 435.8 nm |
| 1.53 @Wavelength 404.7 nm |
| 1.536 @Wavelength 365 nm |
| 1.542 @Wavelength 344.1 nm |
| 1.548 @Wavelength 312.6 nm |
Abbe Number | 63.96 |
| 64.17 |
Optical Dispersion | 0.008054 |
| 0.00811 |
Transmission, Visible | 99.6 % @Thickness 25.0 mm, Wavelength 420 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 436 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 460 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 620 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 660 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 500 nm |
| 99.8 % @Thickness 25.0 mm, Wavelength 546 nm |
| 99.8 % @Thickness 25.0 mm, Wavelength 700 nm |
| 99.8 % @Thickness 25.0 mm, Wavelength 580 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 460 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 436 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 420 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 620 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 580 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 700 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 660 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 546 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 500 nm |
IR Transmittance | 49 % @Thickness 25.0 mm, Wavelength 2500 nm |
| 65.7 % @Thickness 25.0 mm, Wavelength 2325 nm |
| 75.2 % @Thickness 10.0 mm, Wavelength 2500 nm |
| 84.5 % @Thickness 10.0 mm, Wavelength 2325 nm |
| 88.8 % @Thickness 25.0 mm, Wavelength 1970 nm |
| 95.4 % @Thickness 10.0 mm, Wavelength 1970 nm |
| 98.7 % @Thickness 25.0 mm, Wavelength 1530 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 1530 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1060 nm |
| 99.9 % @Thickness 25.0 mm, Wavelength 1060 nm |
UV Transmittance | 2.3 % @Thickness 25.0 mm, Wavelength 300 nm |
| 4.0 % @Thickness 10.0 mm, Wavelength 290 nm |
| 22.1 % @Thickness 10.0 mm, Wavelength 300 nm |
| 24.2 % @Thickness 25.0 mm, Wavelength 310 nm |
| 56.7 % @Thickness 10.0 mm, Wavelength 310 nm |
| 60 % @Thickness 25.0 mm, Wavelength 320 nm |
| 81.5 % @Thickness 10.0 mm, Wavelength 320 nm |
| 87.5 % @Thickness 25.0 mm, Wavelength 334 nm |
| 94.8 % @Thickness 10.0 mm, Wavelength 334 nm |
| 96.4 % @Thickness 25.0 mm, Wavelength 350 nm |
| 98.5 % @Thickness 10.0 mm, Wavelength 350 nm |
| 98.5 % @Thickness 25.0 mm, Wavelength 365 nm |
| 98.9 % @Thickness 25.0 mm, Wavelength 370 nm |
| 99.2 % @Thickness 25.0 mm, Wavelength 380 nm |
| 99.4 % @Thickness 25.0 mm, Wavelength 390 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 365 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 370 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 405 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 400 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 380 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 400 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 390 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 405 nm |
|
Descriptive Properties |
---|
Climatic resistance | 1 |
Grindability | 3 |
Phosphate resistance | 2.3 |
Stress optical coefficient | 2.77 |