MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Mitsubishi Chemical Advanced Materials Ketron™ LSG FG PEEK Poly-ether-ether-ketone
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Unreinforced

Material Notes: Life Science and Food Grade PEEK stock shapes, made from unfilled PEEK resin. Pre-assessed for biocompatibility on both resin and shape for up to 24 hours contact with body tissue according to USP VI and ISO 10993. Some color variations are also pre-assessed for use in wetted contact applications in bioprocessing. Standard food approvals include FDA 21 CFR § 177.2415 and EU 10/2011. Exhibits high mechanical strength and stiffness, and excellent resistance to chemicals and repeated sterilization via all current methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.31 g/ccASTM D792
Water Absorption at Saturation 0.500 %ASTM D570 (17)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 105ASTM D785
Hardness, Shore D 85.0ISO 868
Tensile Strength 115 MPaISO 527-1/-2 (7)
Elongation at Yield 5.00 %ISO 527-1/-2 (7)
Flexural Strength 170 MPaISO 178 (12)
Compressive Yield Strength 38.0 MPa
@Strain 1.00 %
ISO 604 (10)
 75.0 MPa
@Strain 2.00 %
ISO 604 (10)
 140 MPa
@Strain 5.00 %
ISO 604 (10)
Shear Strength 55.0 MPaASTM D732
Charpy Impact, Notched 3.50 kJ/m²ISO 179-1/1eA
 
Electrical PropertiesOriginal ValueComments
Surface Resistivity per Square 1.00e+14 ohmANSI/ESD STM 11.11
Dielectric Constant 3.30
@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 24.0 kV/mmIEC 60243-1 (15)
 480 kV/inASTM D149
Dissipation Factor 0.00300
@Frequency 1.00e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 26.0 µin/in-°FASTM E-831 (TMA)
 50.0 µm/m-°C
@Temperature 23.0 - 100 °C
 55.0 µm/m-°C
@Temperature 23.0 - 150 °C
 130 µm/m-°C
@Temperature >=150 °C
Thermal Conductivity 0.250 W/m-K
 1.75 BTU-in/hr-ft²-°F
Melting Point 644 °FASTM D3418
Maximum Service Temperature, Air 480 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 320 °FASTM D648
Minimum Service Temperature, Air -50.0 °C
 
Compliance PropertiesOriginal ValueComments
FDA Yes
USP Class VI Yes
 
Chemical Resistance PropertiesOriginal ValueComments
Acids, Strong (pH 1-3) Limited
Acids, Weak Acceptable
Alcohols Acceptable
Alkalies, Strong (pH 11-14) Acceptable
Alkalies, Weak Acceptable
Chlorinated Solvents Acceptable
Continuous Sunlight Acceptable
Hot Water / Steam Acceptable
Hydrocarbons - Aliphatic Acceptable
Hydrocarbons - Aromatic Acceptable
Inorganic Salt Solutions Acceptable
Ketones, Esters Acceptable
 
Descriptive Properties
ESd categoryInsulative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

P1SMU757 / 323872

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.