MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Morgan Advanced Ceramics Hicast Extra CR Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Calcined Bauxite raw material base. Hydraulic bond. A low cement, bauxite 1700°C castable with high strengths at all temperatures, low porosity and excellent abrasion, impact and alkali resistance. Chrome addition ensures improved slag/metal contact resistance.

Applications:

  • Forge furnace hearths
  • Door jambs, lintels and piers
  • Cartops
  • Rotary kiln nose rings, retainer rings and dams
  • Rotary hearth curbs
  • Walking beam furnace hearth, pusher furnace hearths
  • Skid pipe protection

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 2.72 g/cc0.0983 lb/in³dried to 110°C
Grain Size <= 6000 µm<= 6000 µm
 
Mechanical PropertiesMetricEnglishComments
Compressive Strength  80.0 MPa
@Treatment Temp. 815 °C
11600 psi
@Treatment Temp. 1500 °F
Cold Crushing Strength
 100 MPa
@Treatment Temp. 1000 °C
14500 psi
@Treatment Temp. 1830 °F
Cold Crushing Strength
 110 MPa
@Treatment Temp. 1600 °C
16000 psi
@Treatment Temp. 2910 °F
Cold Crushing Strength
 120 MPa
@Treatment Temp. 1800 °C
17400 psi
@Treatment Temp. 3270 °F
Cold Crushing Strength
Abrasion >= 6.0
@Temperature 815 °C
>= 6.0
@Temperature 1500 °F
cm3; ASTM C704
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 2.19 W/m-K
@Temperature 600 °C
15.2 BTU-in/hr-ft²-°F
@Temperature 1110 °F
Maximum Service Temperature, Air <= 1700 °C<= 3090 °F
Shrinkage  0.00 - 0.20 %
@Treatment Temp. 815 °C
0.00 - 0.20 %
@Treatment Temp. 1500 °F
 0.10 %
@Treatment Temp. 1000 °C
0.10 %
@Treatment Temp. 1830 °F
 0.30 %
@Treatment Temp. 1600 °C
0.30 %
@Treatment Temp. 2910 °F
 1.9 %
@Treatment Temp. 1800 °C
1.9 %
@Treatment Temp. 3270 °F
 
Component Elements PropertiesMetricEnglishComments
Al2O3 79 %79 %
CaO 1.7 %1.7 %
Cr2O3 1.5 %1.5 %
Fe2O3 1.5 %1.5 %
K2O+Na2O 0.20 %0.20 %Na2O + K2O
MgO 0.40 %0.40 %
SiO2 13 %13 %
TiO2 2.8 %2.8 %
 
Descriptive Properties
Net Material Required (kg/m³)2720
Water Addition5.7-6.7% by weight, 1.425-1.675 L per bag, 25 kg bag weight.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CMORF6334 / 203118

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.