MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Henkel Loctite® Stycast® 2850FT with CAT 9 Two-Component Thermally Conductive Encapsulant
Categories: Polymer; Thermoset; Epoxy; Epoxy Encapsulant, Unreinforced

Material Notes: Loctite Stycast 2850FT provides the following product characteristics:
  • Thermally conductive
  • Electrically insulative
  • Thermal shock resistant
  • Low CTE
  • Can be used with a variety of catalysts

Application: Thermally conductive epoxy encapsulant

Typical Assembly Applications: Encapsulating

Loctite Stycast 2850FT is recommended for encapsulation of components that require heat dissipation and thermal shock properties.

Loctite Stycast 2850FT is also available in the unpigmented version.

Loctite Stycast 2850FT can be used with Loctite CAT 9, Loctite CAT 11, Loctite CAT 23LV or Loctite CAT 24LV

CATALYST DESCRIPTION

Loctite CAT 9 provides the following product characteristics:

  • General purpose
  • Good chemical resistance
  • Good physical strength

Cure: Room temperature cure

Information provided by Henkel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.00 g/cc0.0361 lb/in³Part B, Loctite CAT 9
 2.29 g/cc0.0827 lb/in³Mixed
 2.40 g/cc0.0867 lb/in³Part A, Loctite Stycast 2850FT
Water Absorption 0.030 %
@Time 86400 sec
0.030 %
@Time 24.0 hour
Immersion
Viscosity 92 cP92 cPPart B, Loctite CAT 9
 58000 cP58000 cPMixed
Brookfield Viscosity 250000 cP250000 cPPart A, Loctite Stycast 2850FT; Spindle 7, Speed 10 rpm
 250000 cP250000 cPPart A, Loctite Stycast 2850FT, Small Sample Adapter; Spindle 14, speed 3 rpm
Linear Mold Shrinkage 0.0020 cm/cm0.0020 in/in
Outgassing - Total Mass Loss 0.010 %0.010 %NASA Method, Sample cured 24 hours @ 25ºC; CVCM
 0.25 %0.25 %NASA Method, Sample cured 24 hours @ 25ºC; TML
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 9696
Flexural Strength 92.0 MPa13300 psi
Compressive Strength 155 MPa22500 psi
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cm
Dielectric Constant 5.01
@Frequency 1e+6 Hz
5.01
@Frequency 1e+6 Hz
Dielectric Strength 14.4 kV/mm366 kV/in
Dissipation Factor 0.028
@Frequency 1e+6 Hz
0.028
@Frequency 1e+6 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear 35.0 µm/m-°C19.4 µin/in-°FAlpha 1
 98.9 µm/m-°C54.9 µin/in-°FAlpha 2
Thermal Conductivity 1.25 W/m-K8.68 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 130 °C266 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
Glass Transition Temp, Tg 86.0 °C187 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  60.0 - 120 min
@Temperature 65.0 °C
1.00 - 2.00 hour
@Temperature 149 °F
Option 3. Post cure of 2 to 4 hours at the highest expected use temperature is recommended.
 240 - 360 min
@Temperature 45.0 °C
4.00 - 6.00 hour
@Temperature 113 °F
Option 2. Post cure of 2 to 4 hours at the highest expected use temperature is recommended.
 960 - 1440 min
@Temperature 25.0 °C
16.0 - 24.0 hour
@Temperature 77.0 °F
Option 1. Post cure 2 to 4 hours at the highest expected use temperature is recommended.
Working Life 45.0 min
@Temperature 25.0 °C
45.0 min
@Temperature 77.0 °F
100 g
Shelf Life 12.0 Month12.0 MonthPart A, Loctite Stycast 2850FT
 
Descriptive Properties
AppearanceBlackPart A, Loctite Stycast 2850FT
Mix Ratio, by Volume100 : 8.5Material : Catalyst
Mix Ratio, by Weight100 : 3.5Material : Catalyst

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHENK7930 / 255417

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.