MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

(Viewing data as-entered. Click here to return)
Reynolds MT-13® Epoxy Adhesive Cement
Categories: Polymer; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Product Overview: Smooth-On MT-13® is a premium performance epoxy for applications requiring maximum holding power and water resistance. MT-13® is a two component epoxy adhesive cement which is mixed in equal parts by volume (100A/123B by weight). Pot Life is 35 minutes and handling strength develops in 16 hours at 73° F / 23° C. MT-13® adheres extremely well to both porous and non-porous surfaces. MT-13® is widely used by the boating industry for assembly and general repair. MT-13® also maintains holding power under extreme cold conditions.

Information provided by Reynolds Advanced Materials

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.37 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Barcol 72935
Tensile Strength 4300 psi
Elongation at Break 0.80 %
Modulus of Elasticity 165 ksiCompression
 285 ksiTension
Compressive Yield Strength 8700 psi
Adhesive Bond Strength 900 psi
@Temperature 80.0 °C
Exposure: None; Substrate: AL 2024-T-3; ASTM D1002
 3000 psi
@Temperature -50.0 °C
Exposure: None; Substrate: AL 2024-T-3; ASTM D1002
 3100 psi
@Temperature 25.0 °C
Exposure: None; Substrate: AL 2024-T-3; ASTM D1002
 3100 psi
@Temperature 25.0 °C
Exposure: 30 days in tap water @ 25°C; Substrate: AL 2024-T-3; ASTM D1002
 3100 psi
@Temperature 25.0 °C
Exposure: 7 days in 100% RH @ 65°C; Substrate: AL 2024-T-3; ASTM D1002
 5100 psi
@Temperature 25.0 °C
Exposure: None; Substrate: Cold Rolled Steel; ASTM D1002
 
Processing PropertiesOriginal ValueComments
Cure Time 16.0 hourFull Cure Time
Pot Life 35.0 min
 
Descriptive Properties
ColorWhite
Mix Ratio100A:123Bby weight
 1A:1Bby volume
Mixed ViscosityLight-paste
Sag Resistance1/16”

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PREYN000 / 296701

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.