MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
A. Schulman SCHULAMID® 6 GF15H 30% Glass Fiber Reinforced Nylon 6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled

Material Notes:
Information provided by A. Schulman.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.35 g/ccASTM D792
Linear Mold Shrinkage 0.0020 cm/cm
@Thickness 3.175 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 22900 psiASTM D638
Elongation at Break 5.0 %ASTM D638
Flexural Strength 32000 psiASTM D790
Flexural Modulus 1.279e+6 psiASTM D790
Izod Impact, Notched 2.10 ft-lb/inASTM D256
Izod Impact, Unnotched 15.0 ft-lb/inASTM D4812
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 425 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 396 °FASTM D648
 
Processing PropertiesOriginal ValueComments
Melt Temperature 518 - 563 °F
Mold Temperature 150 - 200 °F
Drying Temperature 175 °F
Dry Time 2 - 4 hourPredrying

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
A. Schulman SCHULAMID® 6 GB30 30% Glass Bead Reinforced Nylon 6
Asahi Kasei Leona™ 54G33 Polyamide 66, GF Reinforced
A. Schulman ComAlloy Hiloy® 612 Nylon 6, Glass Reinforced, UL
A. Schulman ComAlloy® E-16558 30% Glass Fiber Reinforced Nylon
Akro-Plastic Akromid® B3 GF 30 (2472) PA 6 Dry, 30% Glass Filled

PASHU317 / 25281

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.