MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont™ Kapton® 200EN Polyimide Film, 50 Micron Thickness
Categories: Polymer; Film; Thermoset; Polyimide, TS; Polyimide, Thermoset Film

Material Notes: Film thickness 50 micron 2.0 mil)

Kapton® Type E and EN films have superior dimensional stability, low CHE, a CTE close to copper, and a high modulus. This type is exceptional for applications requiring adhesive or adhesiveless constructions.

General Kapton® information: Kapton® is synthesized by polymerizing an aromatic dianhydride with an aromatic diamine. It has excellent chemical resistance; there are no known organic solvents for the film. It does not melt. It can be used at both high and low temperature extremes. Kapton® polyimide films can be used in a variety of electrical and electronic uses: wire and cable tapes, formed coil insulation, substrates for printed circuit boards, motor slot liners, magnet wire insulation, transformer and capacitor insulation, magnetic and pressure-sensitive tapes, and tubing.

Data provided by DuPont High Performance Films.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.46 g/cc
Water Absorption 2.2 %24 hr/23°C. ASTM D570
Thickness 50.0 mil
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 55 %Orientation not specified; ASTM D882
Poissons Ratio 0.34Value for Kapton® HN
Secant Modulus 5.20 GPaASTM D882
Coefficient of Friction, Dynamic 0.48Value for Kapton® HN. Film to film. ASTM D1894-90
Coefficient of Friction, Static 0.63Kapton® HN. Film to film. ASTM D1894-90
Film Tensile Strength at Break, MD 310 MPaOrientation not specified; ASTM D882
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+10 ohm-cmKapton® HN in damp heat; IPC-TM-650; Method 2.5.17
 1.00e+17 ohm-cmper ASTM D257-91 for Kapton® HN
Dielectric Constant 3.2
@Frequency 1000 Hz
Use evaporated metal electrodes, two terminal system of measurement at standard conditions.; ASTM D150
Dielectric Strength 244 kV/mmFlat sheets in air; 1/4 in diameter brass electrodes with 0.8 mm edge radius; 60 cps AC at 600V/s; ASTM D149-81
Dissipation Factor 0.0015
@Frequency 1000 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.0 µm/m-°C
@Temperature 20.0 °C
Value for Kapton® HN
 32.0 µm/m-°C
@Temperature 100 °C
Value for Kapton® HN
 40.0 µm/m-°C
@Temperature 250 °C
Value for Kapton® HN
Specific Heat Capacity 1.09 J/g-°CValue for Kapton® HN
Thermal Conductivity 0.120 W/m-KValue for Kapton® HN
Maximum Service Temperature, Air 400 °CKapton® can function after brief exposure to 400°C (750°F). Various grades are UL rated for continuous service at 220-240°C (430-460°F).
Minimum Service Temperature, Air -269 °CMaintains properties and flexibility
Glass Transition Temp, Tg 385 °CValue for Kapton® HN
Flammability, UL94 V-0
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.70
@Wavelength 589.3 nm
Value for Kapton® HN.  Na D line; ASTM D542-90

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont™ Kapton® 100KN Polyimide Film, 25 Micron Thickness
DuPont™ Kapton® 200HN Polyimide Film, 50 Micron Thickness
DuPont™ Kapton® 200KN Polyimide Film, 50 Micron Thickness
DuPont™ Kapton® 100EN Polyimide Film, 25 Micron Thickness
DuPont™ Kapton® 300KN Polyimide Film, 75 Micron Thickness

PDUK26 / 33396

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.