Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.85 g/cc | 1.85 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 81 | 81 |
| 70 @Treatment Temp. 200 °C, Time 252000 sec | 70 @Treatment Temp. 392 °F, Time 70.0 hour |
| 75 @Treatment Temp. 200 °C, Time 252000 sec | 75 @Treatment Temp. 392 °F, Time 70.0 hour |
| 78 @Treatment Temp. 23.0 °C, Time 252000 sec | 78 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 78 @Treatment Temp. 100 °C, Time 252000 sec | 78 @Treatment Temp. 212 °F, Time 70.0 hour |
| 80 @Treatment Temp. 23.0 °C, Time 252000 sec | 80 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 80 @Treatment Temp. 150 °C, Time 252000 sec | 80 @Treatment Temp. 302 °F, Time 70.0 hour |
| 81 @Treatment Temp. 150 °C, Time 252000 sec | 81 @Treatment Temp. 302 °F, Time 70.0 hour |
| 81 @Treatment Temp. 23.0 °C, Time 252000 sec | 81 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 81 @Treatment Temp. 250 °C, Time 252000 sec | 81 @Treatment Temp. 482 °F, Time 70.0 hour |
| 82 @Treatment Temp. 275 °C, Time 252000 sec | 82 @Treatment Temp. 527 °F, Time 70.0 hour |
Tensile Strength | 16.95 MPa | 2458 psi |
| 12.3207 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 1786.97 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 13.795 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 2000.8 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 13.947 MPa @Treatment Temp. 250 °C, Time 252000 sec | 2022.9 psi @Treatment Temp. 482 °F, Time 70.0 hour |
| 14.405 MPa @Treatment Temp. 200 °C, Time 252000 sec | 2089.3 psi @Treatment Temp. 392 °F, Time 70.0 hour |
| 14.429 MPa @Treatment Temp. 275 °C, Time 252000 sec | 2092.7 psi @Treatment Temp. 527 °F, Time 70.0 hour |
| 14.575 MPa @Treatment Temp. 200 °C, Time 252000 sec | 2113.9 psi @Treatment Temp. 392 °F, Time 70.0 hour |
| 14.897 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2160.6 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 14.95 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2168 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 15.253 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 2212.2 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
Elongation, Ultimate | 260 % | 260 % |
| 210.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 210.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 219.96 % @Treatment Temp. 250 °C, Time 252000 sec | 219.96 % @Treatment Temp. 482 °F, Time 70.0 hour |
| 230.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 230.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 239.98 % @Treatment Temp. 150 °C, Time 252000 sec | 239.98 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 239.98 % @Treatment Temp. 150 °C, Time 252000 sec | 239.98 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 250.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 250.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 260 % @Treatment Temp. 275 °C, Time 252000 sec | 260 % @Treatment Temp. 527 °F, Time 70.0 hour |
| 260 % @Treatment Temp. 200 °C, Time 252000 sec | 260 % @Treatment Temp. 392 °F, Time 70.0 hour |
| 269.9 % @Treatment Temp. 200 °C, Time 252000 sec | 269.9 % @Treatment Temp. 392 °F, Time 70.0 hour |
100% Modulus | 4.98 MPa | 723 psi |
Tear Strength | 27.9 kN/m | 159 pli |
| 28.9 kN/m | 165 pli |
Compression Set | 9.9 % @Treatment Temp. 175 °C, Time 79200 sec | 9.9 % @Treatment Temp. 347 °F, Time 22.0 hour |
| 11.4 % @Treatment Temp. 200 °C, Time 79200 sec | 11.4 % @Treatment Temp. 392 °F, Time 22.0 hour |
| 17.2 % @Treatment Temp. 23.0 °C, Time 79200 sec | 17.2 % @Treatment Temp. 73.4 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -21.1 °C | -6.00 °F |
Shrinkage | 0.20 % @Treatment Temp. 23.0 °C, Time 252000 sec | 0.20 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 0.40 % @Treatment Temp. 150 °C, Time 252000 sec | 0.40 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 1.5 % @Treatment Temp. 23.0 °C, Time 252000 sec | 1.5 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 1.5 % @Treatment Temp. 23.0 °C, Time 252000 sec | 1.5 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 1.8 % @Treatment Temp. 150 °C, Time 252000 sec | 1.8 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 2.8 % @Treatment Temp. 100 °C, Time 252000 sec | 2.8 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 9.7 % @Treatment Temp. 200 °C, Time 252000 sec | 9.7 % @Treatment Temp. 392 °F, Time 70.0 hour |
| 16.8 % @Treatment Temp. 200 °C, Time 252000 sec | 16.8 % @Treatment Temp. 392 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |