MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Master Bond UV26SP One part, UV Curable System
Categories: Polymer; Thermoset

Material Notes: Key Features:
  • Excellent physical strength properties
  • High glass transition temperature
  • Superb chemical resistance
  • No oxygen inhibition
Product Description: Master Bond UV26SP is a one part UV curing system for bonding, sealing and coating. UV26SP cures exceptionally quickly when exposed to UV light emitting at a wavelength of 320-365 nm with an energy output as low as 20-40 milliwatts per cm². UV26SP is highly exothermic. It cures very quickly and should not be cured in sections thicker than .004 to .005 inches. It should be noted that when bonding, a thickness of .001 to .002 inches is more than adequate. Most important, UV26SP is not oxygen inhibited. The system bonds well to glass, surface treated metals, and many plastics including polycarbonates and acrylics. UV26SP is not only effective as an adhesive, but also as a coating and sealant. It is able to withstand acids, bases, fuels, and many aggressive solvents far better than most other UV systems. Its glass transition temperature is 160 to 170°C, considerably higher than other UVs. This system does not contain any solvents or volatiles and features low shrinkage upon curing. Its service temperature range is -60°F to +500°F. UV26SP is a specialty type UV curable with advantageous chemical and temperature resistance, thus, it is a prime candidate for applications in aerospace, electronic, optical, specialty OEM and related industries.

Product Advantages:

  • Fast cure upon exposure to a UV light
  • No oxygen inhibition while curing
  • Very good adhesion to a variety of substrates
  • Outstanding optical clarity
  • Top notch chemical and temperature resistance

Information provided by Master Bond, Inc.

Vendors: Master Bond is a leading manufacturer of adhesives, sealants, coatings and potting compounds. Master Bond’s vast product line consists of over 3,000 epoxy, polyurethane, silicone, cyanoacrylate and latex adhesives that vary in viscosity, cure speed, strength, chemical resistance, electrical properties, etc. Our custom adhesives offer design flexibility and provide excellent bonding performance. Visit www.masterbond.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Viscosity 250 - 1500 cP
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 80.0 - 90.0
Tensile Strength 7000 - 8000 psi
Tensile Modulus 350000 - 400000 psi
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+14 ohm-cm
Dielectric Constant 4.30
@Frequency 60 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 50.0 - 55.0 µm/m-°C
Maximum Service Temperature, Air 260 °C
Minimum Service Temperature, Air -51.0 °C
Glass Transition Temp, Tg 160 - 170 °C
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.55
 
Processing PropertiesOriginal ValueComments
Shelf Life 6.00 Monthin original, unopened containers

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMASTM5814 / 323331

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.