MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Sorona® 3015G BK001 PTT-GF45  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polyester, TP; Polytrimethylene Terephthalate (PTT)

Material Notes: 15% Glass Reinforced Polytrimethylene Terephthalate with Resin Made from Bio-PDO

Information provided by DuPont.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.40 g/ccISO 1183
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 110 MPaISO 527-1/-2
Elongation at Break 2.3 %ISO 527-1/-2
Tensile Modulus 6000 MPaISO 527-1/-2
Flexural Strength 170 MPaISO 178
Flexural Modulus 5700 MPaISO 178
Poissons Ratio 0.35ISO 527-1/-2
Charpy Impact Unnotched 25.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
 25.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 3.00e+14 ohmIEC 62631-3-2
Dielectric Constant 3.9
@Frequency 1e+6 Hz
IEC 62631-2-1
 4.0
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 36.0 kV/mmIEC 60243-1
Dissipation Factor 0.0015
@Frequency 100 Hz
IEC 62631-2-1
 0.017
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 275 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 227 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 215 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 185 °CISO 75-1/-2
Flammability, UL94 HB
@Thickness 0.750 mm
IEC 60695-11-10
 HB
@Thickness 1.50 mm
IEC 60695-11-10
Oxygen Index 21 %ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 250 - 270 °CInjection
 260 °CInjection Optimum
Mold Temperature 80.0 - 110 °CInjection
 100 °CInjection Optimum
Ejection Temperature 175 °CInjection
Drying Temperature 120 °CInjection
Dry Time 2.00 - 4.00 hourDehumidified Dryer; Injection
Moisture Content 0.020 %Injection
 
Descriptive Properties
Back pressureAs low as possibleInjection
Drying RecommendedyesInjection
Part Marking Code>PTT-GF15<ISO 11469
ProcessingInjection Molding

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Sorona® 2045G BK346A PTT-GF45
Overview of materials for Polybutylene Terephthalate (PBT), Extrusion Grade
DuPont Mobility and Materials Sorona® 3030G BK001 PTT-GF30
DuPont Mobility and Materials Sorona® FG3301 NC010 PTT
Overview of materials for Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled

PZDSX5282 / 197922

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.