MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Syensqo (Solvay Specialty Polymers) Ryton® R-4-230BL PPS, 40% glass fiber
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler

Material Notes: 40% glass fiber, low flash, high flow, good strength, black color

Ryton® R-4-230NA and R-4-230BL 40% glass fiber reinforced polyphenylene sulfide compounds provide reduced flash and improved processability compared to other polyphenylene sulfide injection molding compounds.

Applications: Automotive Applications

Features: Good Processability

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.68 g/cc0.0607 lb/in³ASTM D792
Water Absorption 0.020 %
@Time 86400 sec
0.020 %
@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0020 cm/cm
@Thickness 3.20 mm
0.0020 in/in
@Thickness 0.126 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.0050 cm/cm
@Thickness 3.20 mm
0.0050 in/in
@Thickness 0.126 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 104104ASTM D785
Hardness, Rockwell R 122122ASTM D785
Tensile Strength 165 MPa23900 psiASTM D638
Tensile Stress 145 MPa21000 psiISO 527-2
Elongation at Break 1.1 %1.1 %ISO 527-2
 1.2 %1.2 %ASTM D638
Flexural Strength 210 MPa30500 psiISO 178
 221 MPa32100 psiASTM D790
Flexural Modulus 14.0 GPa2030 ksiISO 178
 14.5 GPa2100 ksiASTM D790
Compressive Strength 275 MPa39900 psiASTM D695
Poissons Ratio 0.430.43ASTM E132
Izod Impact, Notched 0.800 J/cm
@Thickness 3.18 mm
1.50 ft-lb/in
@Thickness 0.125 in
ASTM D256
Izod Impact, Unnotched 4.00 J/cm
@Thickness 3.18 mm
7.49 ft-lb/in
@Thickness 0.125 in
ASTM D256
Izod Impact, Notched (ISO) 8.00 kJ/m²3.81 ft-lb/in²Notch A; ISO 180
Izod Impact, Unnotched (ISO) 20.0 kJ/m²9.52 ft-lb/in²ISO 180
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmASTM D257
Surface Resistance 1.00e+16 ohm1.00e+16 ohmASTM D257
Insulation Resistance 1.00e+12 ohm
@Temperature 90.0 °C
1.00e+12 ohm
@Temperature 194 °F
IEC 60167
Dielectric Constant  3.9
@Frequency 1000 Hz
3.9
@Frequency 1000 Hz
ASTM D150
 3.9
@Frequency 1e+6 Hz
3.9
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 20.0 kV/mm508 kV/inASTM D149
Dissipation Factor  0.0020
@Frequency 1000 Hz
0.0020
@Frequency 1000 Hz
ASTM D150
 0.0020
@Frequency 1e+6 Hz
0.0020
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 125 sec125 secASTM D495
Comparative Tracking Index 100 - 174 V100 - 174 VPLC 4; UL 746
 175 V175 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  15.0 µm/m-°C
@Temperature 100 - 200 °C
8.33 µin/in-°F
@Temperature 212 - 392 °F
ASTM E831
 15.0 µm/m-°C
@Temperature -50.0 - 50.0 °C
8.33 µin/in-°F
@Temperature -58.0 - 122 °F
ASTM E831
CTE, linear, Transverse to Flow  40.0 µm/m-°C
@Temperature -50.0 - 50.0 °C
22.2 µin/in-°F
@Temperature -58.0 - 122 °F
ASTM E831
 80.0 µm/m-°C
@Temperature 100 - 200 °C
44.4 µin/in-°F
@Temperature 212 - 392 °F
ASTM E831
Thermal Conductivity 0.310 W/m-K2.15 BTU-in/hr-ft²-°FASTM C177
Maximum Service Temperature, Air 200 - 220 °C392 - 428 °FUL Temperature Rating
Deflection Temperature at 1.8 MPa (264 psi) 265 °C509 °FUnannealed; ASTM D648
Flammability, UL94  V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
 5VA
@Thickness 1.60 mm
5VA
@Thickness 0.0630 in
Oxygen Index 50 %50 %ASTM D2863
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorBlack
FormsPellets
ProcessingInjection Molding
RoHS ComplianceYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4431 / 280231

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.