MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Empilon EMPILON® 795 TPE
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: EMPILON® series can be widely used in general products (such as tool grips, automotive parts, industrial products, sporting goods, etc.) that require high tensile strength, heat resistance and weather resistance. It is mainly a hydrogenated Styrenic Block Copolymer blending materials, hardness range from Shore A16 to Shore D52, can be processed by injection molding, extrusion molding and calendaring. The series is non-toxic. It does not contain RCRA 8 heavy metals, halogens, phthalate and is 100% recyclable and eco-friendly. It can pass the European Union Waste Electronics and Electrical Equipment (WEEE), Restriction of Hazardous Substances (RoHS) regulations and meet the environmental requirements of SONY SS-00259 4th Edition. The series has good chemical resistant and hydrolysis resistant performance.This series can be used without drying before processing. If you want to dye this series of products, please choose PE or EVA as the substrate of masterbatch, never use PVC as the substrate. Moreover, use a higher screw speed when processing and higher back pressure to achieve better dispersion of the colorant.

Series Features:

  • Excellent Mechanical Property and Toughness
  • Excellent Weather Resistance
  • Excellent Heat Aging Resistance
  • Excellent Low Temperature Property
  • Chemical Resistance
  • Hydrolysis Resistance
  • Easy to Processing, apply to general usage product
  • Wide Hardness Range
  • Apply to weather resistant and high strength product
  • Apply to sporting and industrial goods
Applications:
  • Derailleur Cap: Escalate quality
  • Bike Pedals: Aesthetic/Comfortable tactile feeling
  • Scissors Handle: Aesthetic/Comfortable tactile feeling
  • Toy Car Wheel: Comfortable tactile feeling/Wear resistance
  • Comfortable tactile: Comfortable tactile feeling/Good sealing performance
  • Fins: Hydrolysis Resistance/Comfortable tactile feeling

Information provided by EMILON®

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.05 g/ccASTM D792
Melt Flow >= 13 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 52
@Time 10.0 sec
ASTM D2240
Tensile Strength 75.0 kg(f)/cm²ASTM D412
Elongation at Break 450 %ASTM D412
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -50.0 °C
Shrinkage, MD 0.70 %
Shrinkage, TD 1.0 %
 
Processing PropertiesOriginal ValueComments
Feed Temperature 175 - 185 °C
Middle Barrel Temperature 185 - 195 °C
Front Barrel Temperature 190 - 205 °C
Nozzle Temperature 190 - 210 °C
Melt Temperature 175 - 210 °C
 <= 230 °Cdo not exceed
Mold Temperature 30.0 - 50.0 °C
Injection Pressure 3.43 - 4.90 MPa
Back Pressure 0.490 - 0.981 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEMPIL032 / 294719

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.