MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SYNTHOS Krasten® 172 General Purpose Polystyrene
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Heat Resistant Grade

Material Notes: Very good heat resistance and mechanical strength.

Examples of Application:
Extrusion – cups for hot drinks, shower enclosure panels, lightweight XPS sheets. Blends with high impact polystyrene, SBS, thermoformed packaging.
Injection moulding – vegetable boxes for refrigerators, CD and DVD cases.

Synthos was formerly known as Kaucuk. All information provided by Synthos.

Key Words: GPPS
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
Linear Mold Shrinkage 0.0020 - 0.0050 cm/cmInternal; 50x50mm
Melt Flow 2.8 - 3.5 g/10 min
@Load 5.00 kg,
Temperature 200 °C
Granulate; ISO 1133/H
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 150 MPaH 358/30; Ø 50x4mm; ISO 2039-1
Tensile Strength at Break 56.0 MPa5mm/min; ISO 527-2/1A/5
Elongation at Break 3.0 %50mm/min; ISO 527-2/1A/5
Tensile Modulus 3200 MPa1mm/min; ISO 527-2/1A/1
Flexural Strength 100 MPa2mm/min; 80x10x4mm; ISO 178
Izod Impact, Unnotched (ISO) 12.0 kJ/m²
@Temperature 23.0 °C
80x10x4mm; ISO 180/1U
Charpy Impact Unnotched 1.60 J/cm²
@Temperature 23.0 °C
80x10x4mm; ISO 179/1eU
 2.60 J/cm²
@Temperature 23.0 °C
80x10x4mm; ISO 179/1fU
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+16 ohm-cm500V; Ø 93x3mm; IEC 93
Surface Resistance >= 1.00e+15 ohm500V; Ø 93x3mm; IEC 93
Dielectric Constant <= 2.7
@Frequency 50 Hz
500V; Ø 93x3mm; IEC 250
Dielectric Strength >= 60.0 kV/mmTransformer Oil; Ø 93x3mm; IEC 243-1
Dissipation Factor <= 0.0020
@Frequency 50 Hz
500V; Ø 93x3mm; IEC 250
Comparative Tracking Index >= 250 VSolution A; Ø 93x3mm; IEC 112
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C80x10x4mm; ISO 75-2/Af
Vicat Softening Point 101 °C50°C/h; 50N; 10x10x4mm; ISO 306/B50
 105 °C50°C/h; 10N; 10x10x4mm; ISO 306/A50
Flammability, UL94 HB
@Thickness 1.60 mm
Tested in EZÚ Praha
 HB
@Thickness 3.00 mm
Tested in EZÚ Praha
Glow Wire Test 650 °CØ 93x3mm; IEC 695-2-1

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
KKPC Kuhmo GP 150K High Heat Resistant, High Rigidity GPPS
INEOS Styrolution PS 168 N/L GPPS
Ineos Nova 2110 General Purpose Crystal Polystyrene
SYNTHOS Krasten® 152 General Purpose Polystyrene
Axion Polymers Axpoly® PS01 3009 Green General Purpose Polystyrene

PSYNT021 / 82634

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.