MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Polymer Resources TP-FRG15 Polybutylene Terephthalate, 15% Glass Reinforced, Flame Retardant
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled; Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant

Material Notes: Polybutylene Terephthalate, 15% Glass Reinforced, Flame Retardant

Process: Injection Molding
Notes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.

Information provided by Polymer Resources Corporation.

Key Words: UL E113219
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.54 g/ccASTM D792
Linear Mold Shrinkage 0.0050 - 0.0090 cm/cmASTM D955
Melt Flow 10 - 20 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 13000 psiASTM D638
Tensile Strength, Yield 13000 psiASTM D638
Flexural Strength 20000 psiASTM D790
Flexural Modulus 715 ksiASTM D790
Izod Impact, Notched 1.00 ft-lb/in
@Temperature 22.8 °C
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmASTM D257
Dielectric Strength 580 V/milASTM D149
Comparative Tracking Index 250 - 400 VUL 746
Hot Wire Ignition, HWI 7.0 - 15 sec
@Thickness 0.800 mm
UL 746
 15 - 30 sec
@Thickness 1.50 mm
UL 746
 30 - 60 sec
@Thickness 3.00 mm
UL 746
High Amp Arc Ignition, HAI >= 120 arcs
@Thickness 0.800 mm
UL 746
 >= 120 arcs
@Thickness 1.50 mm
UL 746
 >= 120 arcs
@Thickness 3.00 mm
UL 746
High Voltage Arc-Tracking Rate, HVTR 80.0 - 150 mm/minUL 746
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 400 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 345 °FASTM D648
UL RTI, Electrical 266 °F
@Thickness 0.800 mm
UL 746
 266 °F
@Thickness 1.50 mm
UL 746
 266 °F
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical with Impact 266 °F
@Thickness 0.800 mm
UL 746
 266 °F
@Thickness 1.50 mm
UL 746
 266 °F
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical without Impact 248 °F
@Thickness 1.50 mm
UL 746
 248 °F
@Thickness 3.00 mm
UL 746
Flammability, UL94 V-0
@Thickness 0.850 mm
 V-0 - 5VA
@Thickness 3.00 mm
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 460 - 490 °F
Middle Barrel Temperature 470 - 500 °F
Front Barrel Temperature 480 - 510 °F
Melt Temperature 475 - 525 °F
Mold Temperature 160 - 190 °F
Drying Temperature 240 - 250 °F
Dry Time 3.00 - 4.00 hour
Vent Depth 0.000500 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPOLYQ244 / 160768

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.