MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Corning Gorilla® Glass 3 Touch Screen Glass with NDR
Categories: Ceramic; Glass; Optical

Material Notes: Gorilla® Glass 3 with Native Damage Resistance™ (NDR) is an alkali-aluminosilicate thin sheet glass that is better able to survive the real-world events that most commonly cause glass failure. With its core composition, this glass enables improved damage resistance and toughness by helping to prevent the deep chips and scratches that cause glass to break. This glass is widely used in smart phone, tablet, and laptop displays, other touchscreens, optical components, and other high strength glass applications.

Information provided by Corning Incorporated.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.39 g/cc
Thickness 400 - 2000 microns
 
Mechanical PropertiesOriginal ValueComments
Vickers Microhardness 534kgf/mm²; unstrengthened (200 g load)
 649kgf/mm²; strengthened (200 g load)
Modulus of Elasticity 69.3 GPa
Compressive Strength 950 MPaChemically Strengthened to 40 µm Depth
Poissons Ratio 0.22
Fracture Toughness 0.660 MPa-m½
Shear Modulus 28.5 GPa
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 7.19
@Frequency 2.986e+9 Hz
 7.2
@Frequency 2.466e+9 Hz
 7.23
@Frequency 1.977e+9 Hz
 7.26
@Frequency 1.50e+9 Hz
 7.3
@Frequency 9.1e+8 Hz
 7.37
@Frequency 5.990e+8 Hz
 7.38
@Frequency 4.90e+8 Hz
 7.42
@Frequency 3.81e+8 Hz
 7.44
@Frequency 2.72e+8 Hz
 7.48
@Frequency 1.63e+8 Hz
 7.59
@Frequency 5.40e+7 Hz
Dissipation Factor 0.021
@Frequency 4.90e+8 Hz
 0.021
@Frequency 2.72e+8 Hz
 0.022
@Frequency 3.81e+8 Hz
 0.022
@Frequency 5.4e+7 Hz
 0.022
@Frequency 1.63e+8 Hz
 0.023
@Frequency 5.99e+8 Hz
 0.023
@Frequency 9.12e+8 Hz
 0.023
@Frequency 1.499e+9 Hz
 0.023
@Frequency 1.977e+9 Hz
 0.024
@Frequency 2.466e+9 Hz
 0.025
@Frequency 2.986e+9 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.58 µm/m-°C
@Temperature 0.000 - 300 °C
Softening Point 900 °C107.6 Poise
Annealing Point 628 °C1013.2 Poise
Strain Point 574 °C1014.7 Poise
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.50
@Wavelength 590 nm
core glass
 1.51
@Wavelength 590 nm
compression layer
Transmission, Visible >= 91.5 %
@Wavelength 390 - 800 nm
IR Transmittance >= 90 %
@Wavelength 2200 - 2500 nm
 >= 91.5 %
@Wavelength 700 - 2200 nm
UV Transmittance 0.0 %
@Wavelength <=250 nm
 
Descriptive Properties
Photo-elastic Constant31.9 nm/cm/MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Corning Gorilla® Glass 4 Touch Screen Glass
Corning Gorilla® Glass 2
Corning Large Cover Gorilla® Glass Touch Screen Glass
Corning Antimicrobial Gorilla® Glass Touch Screen Glass
Corning Gorilla® Glass 5 Display Glass

CCORNG14b / 178185

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.