MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

A. Schulman SCHULAMID® 66 GF13 13% Glass Fiber Reinforced Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 10% Glass Fiber Filled

Material Notes:
Information provided by A. Schulman.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.21 g/cc1.21 g/ccASTM D792
Linear Mold Shrinkage 0.0070 cm/cm
@Thickness 3.175 mm
0.0070 in/in
@Thickness 0.1250 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 115 MPa16700 psiASTM D638
Elongation at Break 3.0 %3.0 %ASTM D638
Flexural Strength 155 MPa22500 psiASTM D790
Flexural Modulus 5.195 GPa753.5 ksiASTM D790
Izod Impact, Notched 0.641 J/cm1.20 ft-lb/inASTM D256
Izod Impact, Unnotched 4.11 J/cm7.70 ft-lb/inASTM D4812
 
Thermal PropertiesMetricEnglishComments
Melting Point 262 °C504 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 248 °C478 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 244 °C471 °FASTM D648
 
Processing PropertiesMetricEnglishComments
Melt Temperature 290 - 310 °C554 - 590 °F
Mold Temperature 65.6 - 93.3 °C150 - 200 °F
Drying Temperature 79.4 °C175 °F
Dry Time 2 - 4 hour2 - 4 hourPredrying
Moisture Content 0.080 - 0.12 %0.080 - 0.12 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Zytel® 70G13HS1L BK031 PA66-GF13
Chase Plastics CP Pryme® NN113L (Dry) Nylon 66, 13% Glass Fiber Reinforced, Lubricated
A. Schulman SCHULAMID® 66 GF15H 15% Glass Fiber Reinforced, Heat Stabilized Nylon 66
A. Schulman SCHULAMID® 66 GF33 33% Glass Fiber Reinforced Nylon 66
Envalior Akulon® S223-G2U PA66-GF13, Dry, 13% Glass Filled

PASHU325 / 25289

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.