MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC VALOX™ FR 364 PBT (Americas)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: VALOX 364 is an unreinforced, impact modified flame retardant Polybutylene Terephthalate/Polycarbonate (PBT/PC) injection moldable flame grade. It has excellent chemical resistance and a UL94V0@1.47mm and 5VA@3.0mm flame rating. This is a good candidate for outdoor applications in telecommunications enclosures.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.30 g/cc1.30 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 - 0.010 cm/cm
@Thickness 3.20 mm
0.0080 - 0.010 in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse 0.0080 - 0.010 cm/cm
@Thickness 3.20 mm
0.0080 - 0.010 in/in
@Thickness 0.126 in
SABIC method
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 36.0 MPa5220 psi50 mm/min; ASTM D638
Tensile Strength, Yield 46.0 MPa6670 psi50 mm/min; ASTM D638
Elongation at Break 50 %50 %50 mm/min; ASTM D638
Elongation at Yield 5.0 %5.0 %50 mm/min; ASTM D638
Flexural Yield Strength 66.0 MPa9570 psi1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 1.80 GPa261 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 7.47 J/cm14.0 ft-lb/inASTM D256
 4.27 J/cm
@Temperature -40.0 °C
8.00 ft-lb/in
@Temperature -40.0 °F
ASTM D256
 6.94 J/cm
@Temperature -20.0 °C
13.0 ft-lb/in
@Temperature -4.00 °F
ASTM D256
Dart Drop, Total Energy 45.0 J33.2 ft-lbASTM D3763
 44.0 J
@Temperature -20.0 °C
32.5 ft-lb
@Temperature -4.00 °F
ASTM D3763
 47.0 J
@Temperature -40.0 °C
34.7 ft-lb
@Temperature -40.0 °F
ASTM D3763
 
Electrical PropertiesMetricEnglishComments
Arc Resistance 120 - 180 sec120 - 180 secASTM D495
Comparative Tracking Index >= 600 V>= 600 VUL 746A
Hot Wire Ignition, HWI 30 - 60 sec30 - 60 secUL 746A
High Amp Arc Ignition, HAI >= 120 arcs>= 120 arcsUL 746A
High Voltage Arc-Tracking Rate, HVTR 25.4 - 80.0 mm/min1.00 - 3.15 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  95.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
52.8 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 95.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
52.8 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow  98.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
54.4 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 100 µm/m-°C
@Temperature -40.0 - 40.0 °C
55.6 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 103 °C
@Thickness 3.20 mm
217 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 68.0 °C
@Thickness 3.20 mm
154 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 115 °C239 °FRate B/50; ASTM D1525
 122 °C252 °FRate B/120; ISO 306
UL RTI, Electrical 75.0 °C167 °FUL 746B
UL RTI, Mechanical with Impact 75.0 °C167 °FUL 746B
UL RTI, Mechanical without Impact 75.0 °C167 °FUL 746B
Flammability, UL94  V-0
@Thickness 1.47 mm
V-0
@Thickness 0.0579 in
UL 94
 5VA
@Thickness 2.99 mm
5VA
@Thickness 0.118 in
UL 94
Oxygen Index 28 %28 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 245 - 260 °C473 - 500 °FInjection Molding
Zone 1 240 - 255 °C464 - 491 °F
Zone 2 245 - 260 °C473 - 500 °F
Zone 3 250 - 265 °C482 - 509 °F
Melt Temperature 250 - 265 °C482 - 509 °F
Mold Temperature 50.0 - 75.0 °C122 - 167 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 12.0 hour12.0 hourCumulative; Injection Molding
Moisture Content 0.020 %0.020 %
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 80 %40 - 80 %
Vent Depth 0.00250 - 0.00380 cm0.000984 - 0.00150 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
UV-light, water exposure/immersionF2UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI10316 / 243783

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.