MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SABIC VALOX™ PDR4922 PBT (Asia)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: GF filled PBT grade

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.40 g/ccASTM D792
Density 1.40 g/ccISO 1183
Water Absorption 0.030 %23°C/sat; ISO 62
Moisture Absorption 0.0300 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0016 cm/cm
@Thickness 3.20 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.0094 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 12 g/10 min
@Load 2.16 kg,
Temperature 250 °C
cm³/10 min; ISO 1133
 13.4 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 81.0 MPa50 mm/min; ASTM D638
 81.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 85.0 MPa50 mm/min; ASTM D638
 85.0 MPa50 mm/min; ISO 527
Elongation at Break 3.3 %50 mm/min; ASTM D638
 3.6 %50 mm/min; ISO 527
Elongation at Yield 2.4 %50 mm/min; ASTM D638
 3.0 %50 mm/min; ISO 527
Tensile Modulus 5230 MPa1mm/min; ISO 527
 5410 MPa50 mm/min; ASTM D638
Flexural Yield Strength 130 MPa2 mm/min; ISO 178
 133 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 4580 MPa1.3 mm/min, 50 mm span; ASTM D790
 4860 MPa2 mm/min; ISO 178
Izod Impact, Notched 102 J/mASTM D256
 58.0 J/m
@Temperature -30.0 °C
ASTM D256
Izod Impact, Notched (ISO) 10.0 kJ/m²80*10*4; ISO 180/1A
 6.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Charpy Impact, Notched 8.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 8.00 JASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 41.8 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 43.9 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 114 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 118 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 216 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 170 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 184 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 195 °CRate B/50; ISO 306
 196 °CRate B/120; ISO 306
 200 °CRate B/50; ASTM D1525
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 245 - 260 °CInjection Molding
Zone 1 240 - 255 °C
Zone 2 245 - 260 °C
Zone 3 250 - 265 °C
Melt Temperature 250 - 265 °C
Mold Temperature 50.0 - 75.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 12.0 hourCumulative; Injection Molding
Moisture Content 0.020 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 80 %
Vent Depth 0.00250 - 0.00380 cm
Screw Speed 50 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10287 / 243754

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.