MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Copper, UNS C19700, H06 Temper
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Excellent soldering and brazing. Excellent capacity for both cold and hot forming.

Applications: Electrical and electronic connectors, circuit breaker components, fuse clips, cable shielding, and lead frames. Generally suited to applications requiring excellent formability combined with high strength and conductivity.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.83 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 73
Tensile Strength, Ultimate 480 MPa
Tensile Strength, Yield 470 MPaStrip
Elongation at Break 3.0 %In 50 mm
Modulus of Elasticity 121 GPa
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000216 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.8 µm/m-°C
@Temperature 20.0 - 100 °C
 18.8 µm/m-°C
@Temperature 20.0 - 200 °C
 19.3 µm/m-°C
@Temperature 20.0 - 300 °C
Thermal Conductivity 320 W/m-K
Melting Point 1069 - 1086 °C
Solidus 1069 °C
Liquidus 1086 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 450 - 600 °C
Hot-Working Temperature 750 - 950 °C
 
Component Elements PropertiesOriginal ValueComments
Cobalt, Co <= 0.050 %
Copper, Cu 99.15 %
Iron, Fe 0.30 - 1.2 %
Lead, Pb <= 0.050 %
Magnesium, Mg 0.010 - 0.20 %
Manganese, Mn <= 0.050 %
Phosphorus, P 0.10 - 0.40 %
Tin, Sn <= 0.20 %
Zinc, Zn <= 0.20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
High Strength Modified Copper, UNS C19400, O50 Temper flat products
Johnson Matthey Pallabraze™ 1090 Palladium Based Brazing Alloy
High-Conductivity Oxygen-Free Copper hardened 0.015-0.040 mm grain size
High Strength Modified Copper, UNS C19400, O82 Temper flat products
High Strength Modified Copper, UNS C19400, O60 Temper flat products

MC19700b3 / 10976

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.