MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Norplex-Micarta ShotBlocker NP525 Phenolic Glass Laminate Sheet  (discontinued **)
Categories: Polymer; Thermoset; Phenolic

Material Notes: NP525 is a member of the ShotBlocker™ family of products. Being a high performance composite manufactured from AGY Quicksilver™ R Glass reinforcement with a high-temperature phenolic resin system, NP525 was developed to comply with stringent Military requirements as a ballistic resistant material. NP525 complies with MIL-DTL-64154 Class B Code 2.

Information provided by Norplex-Micarta

Key Words: Glass Fiber, Phenolic, Micarta, MIL-DTL-64154B Class B Code 2, R Glass, Ballistic
Vendors: Norplex-Micarta is the leading manufacturer of high performance thermoset composite materials. We work directly with customers to manufacture the highest quality specialty sheet products, pre-pregs, rods and molded shapes, and tubes to meet demanding composite applications for our OEMs and fabricators around the world. Visit norplex-micarta.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.06 g/cc
@Thickness 12.7 mm
2.06 g/cc
@Thickness 0.500 in
ASTM D792
Moisture Absorption 1.60 %
@Thickness 12.7 mm
1.60 %
@Thickness 0.500 in
ASTM D570 Condition A
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 96
@Thickness 6.35 mm
96
@Thickness 0.250 in
ASTM D785
Tensile Strength  412 MPa
@Thickness 12.7 mm
59800 psi
@Thickness 0.500 in
CrossWise; ASTM D638 Condition A
 453 MPa
@Thickness 12.7 mm
65700 psi
@Thickness 0.500 in
LengthWise; ASTM D638 Condition A
Flexural Strength  179 MPa
@Thickness 12.7 mm
26000 psi
@Thickness 0.500 in
CrossWise; ASTM D790 Condition A
 211 MPa
@Thickness 12.7 mm
30600 psi
@Thickness 0.500 in
LengthWise; ASTM D790 Condition A
Flexural Modulus  26.8 GPa
@Thickness 12.7 mm
3890 ksi
@Thickness 0.500 in
CrossWise; ASTM D790 Condition A
 28.1 GPa
@Thickness 12.7 mm
4070 ksi
@Thickness 0.500 in
LengthWise; ASTM D790 Condition A
Compressive Strength 648 MPa
@Thickness 12.7 mm
94000 psi
@Thickness 0.500 in
Flatwise; ASTM D695 Condition A
Shear Strength 310 MPa
@Thickness 12.7 mm
44900 psi
@Thickness 0.500 in
perpendicular; ASTM D732 Condition A
Izod Impact, Unnotched  21.8 J/cm
@Thickness 12.7 mm
40.9 ft-lb/in
@Thickness 0.500 in
CrossWise; ASTM D256 Condition E-48/50
 21.9 J/cm
@Thickness 12.7 mm
41.1 ft-lb/in
@Thickness 0.500 in
LengthWise; ASTM D256 Condition E-48/50
 
Electrical PropertiesMetricEnglishComments
Dielectric Breakdown 39000 V
@Thickness 12.7 mm
39000 V
@Thickness 0.500 in
ASTM D149 Condition A
 
Thermal PropertiesMetricEnglishComments
UL RTI, Electrical 210 °C410 °FUL Bulletin 746b
UL RTI, Mechanical with Impact 150 °C302 °FUL Bulletin 746b
Flammability, UL94 V-0
@Thickness 12.7 mm
V-0
@Thickness 0.500 in
 
Descriptive Properties
Bonding Strength650[lb]; 0.5"; ASTM D229 Condition D-48/50

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Norplex-Micarta RT342 Phenolic Cotton Laminate Tube, NEMA C
Norplex-Micarta RTB320S Phenolic Linen Laminate Tube, NEMA LE
Norplex-Micarta RT130X Epoxy Fiber Glass Laminate Tube, NEMA FR-4
Norplex-Micarta RT342H Phenolic Cotton Laminate Tube, NEMA C
Norplex-Micarta RTB320H Phenolic Linen Laminate Tube, NEMA LE

PNORPM066 / 192823

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.