MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Teknor Apex Telcar® TL-4001-E Thermoplastic Elastomer
Categories: Polymer; Thermoplastic

Material Notes: Telcar TL-4001-E is a general purpose thermoplastic elastomer designed for the industrial market, including weatherstripping. It is a medium density, medium hardness, UV stable grade that is suitable for injection molding and extrusion.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Filled; Light Stabilized; Medium Density; Medium Hardness; Low Flow; Slip; Sunlight Resistant; UV Absorbing

Uses: General Purpose; Industrial Applications; Weatherstripping

RoHS Compliant:RoHS

Form: Pellets

Processing Method: Injection Molding; Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ASTM D792
Melt Flow 4.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
4.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  70
@Time 5.00 sec
70
@Time 0.00139 hour
Injection Molded; ASTM D2240
 72
@Time 1.00 sec
72
@Time 0.000278 hour
Injection Molded; ASTM D2240
Tensile Strength at Break 5.83 MPa846 psiFlow, Die C, 20 in/min; ASTM D412
 9.72 MPa1410 psiAcross Flow, Die C, 20 in/min; ASTM D412
Tensile Stress at Strain  2.93 MPa
@Strain 100 %
425 psi
@Strain 100 %
Across Flow, Die C, 20 in/min; ASTM D412
 3.79 MPa
@Strain 300 %
550 psi
@Strain 300 %
Across Flow, Die C, 20 in/min; ASTM D412
 5.47 MPa
@Strain 100 %
793 psi
@Strain 100 %
Flow, Die C, 20 in/min; ASTM D412
Elongation at Break 230 %230 %Flow, Die C, 20 in/min; ASTM D412
 1800 %1800 %Across Flow, Die C, 20 in/min; ASTM D412
Tear Strength 40.1 kN/m229 pliFlow, Die C, 20 in/min; ASTM D624
 43.3 kN/m247 pliAcross Flow, Die C, 20 in/min; ASTM D624
Compression Set  35 %
@Temperature 22.8 °C,
Time 79200 sec
35 %
@Temperature 73.0 °F,
Time 22.0 hour
Type 1; ASTM D395B
 65 %
@Temperature 70.0 °C,
Time 79200 sec
65 %
@Temperature 158 °F,
Time 22.0 hour
Type 1; ASTM D395B
 
Processing PropertiesMetricEnglishComments
Processing Temperature 188 - 210 °C370 - 410 °FInjection, Melt
Rear Barrel Temperature 171 - 193 °C340 - 380 °FInjection
Middle Barrel Temperature 177 - 199 °C350 - 390 °FInjection
Front Barrel Temperature 182 - 204 °C360 - 400 °FInjection
Nozzle Temperature 188 - 210 °C370 - 410 °FInjection
Zone 1 166 - 188 °C330 - 370 °FExtrusion
Zone 2 171 - 193 °C340 - 380 °FExtrusion
Zone 3 177 - 199 °C350 - 390 °FExtrusion
Zone 5 182 - 204 °C360 - 400 °FExtrusion
Die Temperature 190 - 210 °C374 - 410 °FExtrusion
Mold Temperature 25.0 - 65.6 °C77.0 - 150 °FInjection
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psiInjection
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psiInjection
Cushion 0.381 - 2.54 cm0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpm30 - 100 rpmExtrusion
 50 - 100 rpm50 - 100 rpmInjection
 
Descriptive Properties
AppearanceColors Available
 Opaque
 White

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1671 / 238162

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.