MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay FM® 300-2K Film Adhesive, psf 0.1 (489 gsm)
Categories: Polymer; Adhesive; Film

Material Notes: Description: FM® 300-2 film adhesive is a 250°F (121°C) cure version of Cytec Engineered Materials’ widely used FM® 300 film adhesive. It delivers the same superior high temperature performance, toughness and stress/strain properties of FM 300 film adhesive without requiring a 350°F (177°C) cure cycle. In addition, FM 300-2 film adhesive’s processing window includes temperatures up to 300°F (149°C) providing a unique level of flexibility from one adhesive product. FM 300-2 adhesive was developed specifically for co-cure and secondary composite bonding applications. Through innovative curative technology, the required cure temperature is reduced allowing for secondary bonding of structure far below the composite’s glass transition point. FM 300-2 film adhesive also offers optimum flow control desirable for co-cure composite bonding. In metal bond applications, FM 300-2 film adhesive provides excellent moisture and corrosion resistance in high humidity environments with a minimal reduction in mechanical properties. To achieve consistent mechanical performance as well as maximum environmental resistance in bonding metallic details, the use of pre-cured BR® 127 corrosion inhibiting primer is recommended. FM 300-2 adhesive is available as an unsupported or supported film employing both knit and random mat carriers. A low-flow version of FM 300-2 film adhesive for composite interleaving, designated FM 300-2 interleaf adhesive, is also available.

Features & Benefits:

  • 250°F (121°C) cure version of FM 300 film adhesive
  • Offers service temperatures from 67°F to 300°F (-55°C to 149°C)
  • Excellent moisture and corrosion resistance in high humidity environments with no significant reduction in mechanical properties
  • Displays similar stress/strain properties to FM 300 film adhesive under both dry and wet conditions through 220°F (104°C)
  • Ideal for co-cure and secondary composite bonding applications. Compatible with most thermoset and thermoplastic composite systems.
Applications:
  • Co-cure and secondary composite bonding
  • Vacuum-only processing common in repair applications

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Volatiles <= 1.0 %
Outgassing - Total Mass Loss 1.35 %TWL
Collected Volatile Condensable Material 0.080 %
Storage Temperature -18.0 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 545 psi
@Temperature 82.0 °C
Flatwise, Immersed in water for 24 hours at 140°F (60°C), then bonded within two hours, Bonded Exposure: 30 days at 160°F (71°C), 100% RH
 570 psi
@Temperature 82.0 °C
Flatwise, 3 weeks at 75°F (24°C), 65% RH, Bonded Exposure: 30 days at 160°F (71°C), 100% RH
 620 psi
@Temperature 121 °C
Flatwise, Immersed in water for 24 hours at 140°F (60°C), then bonded within two hours
 630 psi
@Temperature 121 °C
Flatwise, 3 weeks at 75°F (24°C), 65% RH
 700 psi
@Temperature 121 °C
Flatwise
 700 psi
@Temperature 24.0 °C
Flatwise, 3 weeks at 75°F (24°C), 65% RH, Bonded Exposure: 30 days at 160°F (71°C), 100% RH
 720 psi
@Temperature 24.0 °C
Flatwise, Immersed in water for 24 hours at 140°F (60°C), then bonded within two hours
 730 psi
@Temperature 24.0 °C
Flatwise, Immersed in water for 24 hours at 140°F (60°C), then bonded within two hours, Bonded Exposure: 30 days at 160°F (71°C), 100% RH
 750 psi
@Temperature 82.0 °C
Flatwise, Immersed in water for 24 hours at 140°F (60°C), then bonded within two hours
 780 psi
@Temperature 82.0 °C
Flatwise, 3 weeks at 75°F (24°C), 65% RH
 780 psi
@Temperature 24.0 °C
Flatwise, 3 weeks at 75°F (24°C), 65% RH
 1000 psi
@Temperature 82.0 °C
Flatwise
 1230 psi
@Temperature -55.0 °C
Flatwise
 1240 psi
@Temperature 24.0 °C
Flatwise
Shear Strength 1550 psi
@Temperature 121 °C
Lap, Bonded Exposure: 30 days at 160°F (71°C), 100% RH, 100% Cohesive Failure
 1820 psi
@Temperature 149 °C
Lap, Precured Composite Substrate: PEEK (APC™-2)
 2300 psi
@Temperature 149 °C
Lap, Baseline
 2340 psi
@Temperature 121 °C
Lap, 85% Adhesive Failure, 15% cohesive Failure
 2420 psi
@Temperature 24.0 °C
Lap, 70% Cohesive Failure, 30% Laminate Failure
 2570 psi
@Temperature 82.0 °C
Lap, 60% Cohesive Failure, 40% Laminate Failure
 2600 psi
@Temperature 82.0 °C
Lap, Bonded Exposure: 30 days at 160°F (71°C), 100% RH, 50% Cohesive Failure, 50% Laminate Failure
 2600 psi
@Temperature 24.0 °C
Lap, Bonded Exposure: 30 days at 160°F (71°C), 100% RH, 100% Laminate Failure
 3100 psi
@Temperature -55.0 °C
Lap, Precured Composite Substrate: PEEK (APC™-2)
 3170 psi
@Temperature 82.0 °C
Lap, wet, Precured Composite Substrate: PEEK (APC™-2)
 3650 psi
@Temperature 24.0 °C
Lap, Precured Composite Substrate: PEEK (APC™-2)
 3750 psi
@Temperature 121 °C
Lap; ASTM D1002
 3900 psi
@Temperature 121 °C
Lap, Baseline
 4280 psi
@Temperature -55.0 °C
Lap; ASTM D1002
 4560 psi
@Temperature 107 °C
Lap, Cure Cycle 60 minutes 350°F (177°C)
 4660 psi
@Temperature 107 °C
Lap, Cure Cycle 90 minutes 250°F (121°C)
 4680 psi
@Temperature 107 °C
Lap, Cure Cycle 60 minutes 300°F (149°C)
 5200 psi
@Temperature 82.0 °C
Lap; ASTM D1002
 5410 psi
@Temperature 24.0 °C
Lap; ASTM D1002
 5600 psi
@Temperature 24.0 °C
Lap, Baseline
 6100 psi
@Temperature 24.0 °C
Lap, Cure Cycle 90 minutes 250°F (121°C)
 6280 psi
@Temperature 24.0 °C
Lap, Cure Cycle 60 minutes 350°F (177°C)
 6460 psi
@Temperature 24.0 °C
Lap, Cure Cycle 60 minutes 300°F (149°C)
Peel Strength 36.0 pliFloating Roller
 30.0 pli
@Temperature 24.0 °C
Floating Roller, Cure Cycle 90 minutes 250°F (121°C)
 34.0 pli
@Temperature 24.0 °C
Floating Roller, Cure Cycle 60 minutes 300°F (149°C)
 34.0 pli
@Temperature 24.0 °C
Floating Roller, Cure Cycle 60 minutes 350°F (177°C)
 35.0 pli
@Temperature 24.0 °C
Floating Roller, Bonded Exposure: 30 days at 160F (71C), 100% RH
 35.0 pli
@Temperature 24.0 °C
Floating Roller, Pre-Bond Film Exposure:15 days at 75°F (24°C), 80% RH, Bonded Exposure: 30 days at 160°F (71°C), 100% RH
 36.0 pli
@Temperature 24.0 °C
Floating Roller, Pre-Bond Film Exposure
 36.0 pli
@Temperature 121 °C
Floating Roller, Pre-Bond Film Exposure
 37.0 pli
@Temperature 121 °C
Floating Roller, Pre-Bond Film Exposure:15 days at 75°F (24°C), 80% RH
 39.0 pli
@Temperature 121 °C
Floating Roller, Bonded Exposure: 30 days at 160F (71C), 100% RH
 39.0 pli
@Temperature 121 °C
Floating Roller, Pre-Bond Film Exposure:15 days at 75°F (24°C), 80% RH, Bonded Exposure: 30 days at 160°F (71°C), 100% RH
 40.0 pli
@Temperature 24.0 °C
Floating Roller, Pre-Bond Film Exposure:15 days at 75°F (24°C), 80% RH
 43.0 pli
@Temperature 107 °C
Floating Roller, Cure Cycle 90 minutes 250°F (121°C)
 45.0 pli
@Temperature 107 °C
Floating Roller, Cure Cycle 60 minutes 300°F (149°C)
 49.0 pli
@Temperature 107 °C
Floating Roller, Cure Cycle 60 minutes 350°F (177°C)
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 149 °C
Minimum Service Temperature, Air -55.0 °C
Glass Transition Temp, Tg 140 °CLap, Cure Cycle 60 minutes 300°F (149°C)
 140 °CLap, Cure Cycle 60 minutes 350°F (177°C)
 143 °CLap, Cure Cycle 90 minutes 250°F (121°C)
 144 °C
 
Processing PropertiesOriginal ValueComments
Shelf Life 12.0 Month
 
Descriptive Properties
ColorRed
Honeycomb Sandwich Peel53 Nm/m-55°C
 74 Nm/m24°C
 74 Nm/m121°C
Metal-to-Metal Climbing Drum Peel150 Nm/m24°C
 170 Nm/m82°C
 170 Nm/m121°C
 71 Nm/mCure Cycle 90 minutes 250°F (121°C), 24°C
 74 Nm/mCure Cycle 90 minutes 250°F (121°C), 107°C
 74 Nm/mCure Cycle 60 minutes 350°F (177°C), 24°C
 76 Nm/m-55°C
 77 Nm/mCure Cycle 60 minutes 300°F (149°C), 24°C
 81 Nm/mCure Cycle 60 minutes 300°F (149°C), 107°C
 89 Nm/mCure Cycle 60 minutes 350°F (177°C), 107°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay FM® 300-2K Film Adhesive, psf 0.08 (391 gsm)
Solvay FM® 73U Epoxy Film Adhesive
Phosphorus (V) Sulfide Trifluoride, PSF3
Mitsui MILEX™ XL-1210MB Phenol Aralkyl Resin, Silicone Rubber Modified
Momentive Performance Materials FQE205U Heat Cured Fluorosilicone Rubber

PCYTED112 / 180414

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.